JP2018085420A - Capacitor and method for manufacturing the same - Google Patents

Capacitor and method for manufacturing the same Download PDF

Info

Publication number
JP2018085420A
JP2018085420A JP2016227185A JP2016227185A JP2018085420A JP 2018085420 A JP2018085420 A JP 2018085420A JP 2016227185 A JP2016227185 A JP 2016227185A JP 2016227185 A JP2016227185 A JP 2016227185A JP 2018085420 A JP2018085420 A JP 2018085420A
Authority
JP
Japan
Prior art keywords
solid electrolyte
electrolyte layer
capacitor
mass
poly
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
JP2016227185A
Other languages
Japanese (ja)
Other versions
JP6820727B2 (en
Inventor
鈴木 健一
Kenichi Suzuki
健一 鈴木
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Shin Etsu Polymer Co Ltd
Shin Etsu Chemical Co Ltd
Original Assignee
Shin Etsu Polymer Co Ltd
Shin Etsu Chemical Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Shin Etsu Polymer Co Ltd, Shin Etsu Chemical Co Ltd filed Critical Shin Etsu Polymer Co Ltd
Priority to JP2016227185A priority Critical patent/JP6820727B2/en
Publication of JP2018085420A publication Critical patent/JP2018085420A/en
Application granted granted Critical
Publication of JP6820727B2 publication Critical patent/JP6820727B2/en
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

PROBLEM TO BE SOLVED: To provide: a capacitor which is smaller, in equivalent series resistance, than a conventional one; and a method for manufacturing the capacitor.SOLUTION: A capacitor 10 of the present invention comprises: an anode 11 composed of a porous body of a valve metal; a dielectric layer 12 including an oxide of the valve metal; a cathode 13 made of a conductive material and provided on the opposite side of the dielectric layer 12 to the anode 11; and at least one solid electrolyte layer 14 formed between the dielectric layer 12 and cathode 13. The solid electrolyte layer 14 includes: a conductive complex comprising a π-conjugated conductive polymer and polyanion; and a particular azine compound.SELECTED DRAWING: Figure 1

Description

本発明は、π共役系導電性高分子を含む固体電解質層を備えたキャパシタ及びその製造方法に関する。   The present invention relates to a capacitor including a solid electrolyte layer containing a π-conjugated conductive polymer and a method for manufacturing the same.

キャパシタにおいては、誘電体層と陰極との間に配置される電解質として、導電性高分子を含む固体電解質層を用いて、等価直列抵抗を小さくしたものが知られている。
導電性高分子を含む固体電解質層としては、ポリ(3,4−エチレンジオキシチオフェン)とポリスチレンスルホン酸を含む導電性高分子分散液から形成したものが使用されることがある(例えば、特許文献1)。
As a capacitor, a capacitor in which an equivalent series resistance is reduced by using a solid electrolyte layer containing a conductive polymer as an electrolyte disposed between a dielectric layer and a cathode is known.
As the solid electrolyte layer containing a conductive polymer, a layer formed from a conductive polymer dispersion containing poly (3,4-ethylenedioxythiophene) and polystyrenesulfonic acid may be used (for example, patents). Reference 1).

特開2014−67949号公報JP 2014-67949 A

導電性高分子分散液を用いて製造された従来のキャパシタには、その等価直列抵抗をさらに小さくすることが求められている。
本発明は、等価直列抵抗が従来よりも小さいキャパシタ及びその製造方法を提供する。
A conventional capacitor manufactured using a conductive polymer dispersion is required to further reduce its equivalent series resistance.
The present invention provides a capacitor having a smaller equivalent series resistance than the conventional one and a method for manufacturing the same.

[1] 弁金属の多孔質体からなる陽極と、前記弁金属の酸化物からなる誘電体層と、前記誘電体層の、前記陽極と反対側に設けられた導電物質製の陰極と、前記誘電体層及び前記陰極の間に設けられた少なくとも1層の固体電解質層とを具備し、前記固体電解質層が、π共役系導電性高分子及びポリアニオンを含む導電性複合体と、下記式(1)で表されるアジン化合物とを含有する、キャパシタ。 [1] An anode made of a porous body of a valve metal, a dielectric layer made of an oxide of the valve metal, a cathode made of a conductive material provided on the opposite side of the dielectric layer from the anode, And at least one solid electrolyte layer provided between the dielectric layer and the cathode, wherein the solid electrolyte layer includes a conductive composite containing a π-conjugated conductive polymer and a polyanion, and the following formula ( A capacitor containing the azine compound represented by 1).

Figure 2018085420
[式(1)中、X,X,Xは各々独立してCH又はNであり、R,R,Rは各々独立して水素原子又は任意の置換基であり、X,X,Xのうち少なくとも何れか1つはNであり、R,R,Rのうち少なくとも何れか1つは窒素を有する置換基である。]
[2] 前記固体電解質層は、前記誘電体層の少なくとも一部を覆う第一の固体電解質層と、前記第一の固体電解質層の少なくとも一部を覆う第二の固体電解質層と、を有する、[1]に記載のキャパシタ。
[3] 前記第一の固体電解質層は前記アジン化合物を含み、前記第二の固体電解質層は前記導電性複合体を含む、[2]に記載のキャパシタ。
[4] 前記固体電解質層が、前記式(1)に該当しない含窒素化合物をさらに含有する、[1]〜[3]の何れか一項に記載のキャパシタ。
[5] 前記式(1)に該当しない前記含窒素化合物が、イミダゾール、トリエチルアミン、及びトリプロピルアミンから選ばれる何れか1つ以上である、[4]に記載のキャパシタ。
[6] 前記式(1)中、R,R,Rのうち少なくとも何れか1つはアミノ基である、[1]〜[5]の何れか一項に記載のキャパシタ。
[7] 前記π共役系導電性高分子が、ポリ(3,4−エチレンジオキシチオフェン)である、[1]〜[6]の何れか一項に記載のキャパシタ。
[8] 前記ポリアニオンが、ポリスチレンスルホン酸である、[1]〜[7]の何れか一項に記載のキャパシタ。
[9] 弁金属の多孔質体からなる陽極の表面を酸化して誘電体層を形成する工程と、前記誘電体層に対向する位置に陰極を配置する工程と、前記誘電体層の表面の少なくとも一部に、前記式(1)で表されるアジン化合物を含む溶液を塗布し、乾燥させて、第一の固体電解質層を形成する工程と、前記第一の固体電解質層の表面の少なくとも一部に、π共役系導電性高分子及びポリアニオンを含む導電性複合体が分散された導電性高分子分散液を塗布し、乾燥させて、第二の固体電解質層を形成する工程と、を有するキャパシタの製造方法。
[10] 前記溶液及び前記導電性高分子分散液のうち少なくとも一方が、前記式(1)に該当しない含窒素化合物を含む、[9]に記載のキャパシタの製造方法。
[11] 前記式(1)に該当しない前記含窒素化合物が、イミダゾール、トリエチルアミン、及びトリプロピルアミンから選ばれる何れか1つ以上である、[10]に記載のキャパシタの製造方法。
[12] 前記式(1)中、R,R,Rのうち少なくとも何れか1つはアミノ基である、[9]〜[11]の何れか一項に記載のキャパシタの製造方法。
[13] 前記π共役系導電性高分子が、ポリ(3,4−エチレンジオキシチオフェン)である、[9]〜[12]の何れか一項に記載のキャパシタの製造方法。
[14] 前記ポリアニオンが、ポリスチレンスルホン酸である、[9]〜[13]の何れか一項に記載のキャパシタの製造方法。
Figure 2018085420
[In the formula (1), X 1 , X 2 and X 3 are each independently CH or N, R 1 , R 2 and R 3 are each independently a hydrogen atom or an arbitrary substituent; At least one of 1 , X 2 and X 3 is N, and at least one of R 1 , R 2 and R 3 is a nitrogen-containing substituent. ]
[2] The solid electrolyte layer includes a first solid electrolyte layer covering at least a part of the dielectric layer, and a second solid electrolyte layer covering at least a part of the first solid electrolyte layer. The capacitor according to [1].
[3] The capacitor according to [2], wherein the first solid electrolyte layer includes the azine compound, and the second solid electrolyte layer includes the conductive composite.
[4] The capacitor according to any one of [1] to [3], wherein the solid electrolyte layer further contains a nitrogen-containing compound not corresponding to the formula (1).
[5] The capacitor according to [4], wherein the nitrogen-containing compound not corresponding to the formula (1) is any one or more selected from imidazole, triethylamine, and tripropylamine.
[6] The capacitor according to any one of [1] to [5], wherein at least one of R 1 , R 2 , and R 3 in the formula (1) is an amino group.
[7] The capacitor according to any one of [1] to [6], wherein the π-conjugated conductive polymer is poly (3,4-ethylenedioxythiophene).
[8] The capacitor according to any one of [1] to [7], wherein the polyanion is polystyrene sulfonic acid.
[9] A step of oxidizing a surface of an anode made of a valve metal porous body to form a dielectric layer; a step of disposing a cathode at a position facing the dielectric layer; and a step of forming a surface of the dielectric layer. Applying at least a part of the solution containing the azine compound represented by the formula (1) and drying to form a first solid electrolyte layer; at least a surface of the first solid electrolyte layer; Applying a conductive polymer dispersion in which a conductive complex containing a π-conjugated conductive polymer and a polyanion is dispersed to a part and drying to form a second solid electrolyte layer; A method for manufacturing a capacitor.
[10] The method for producing a capacitor according to [9], wherein at least one of the solution and the conductive polymer dispersion contains a nitrogen-containing compound not corresponding to the formula (1).
[11] The method for manufacturing a capacitor according to [10], wherein the nitrogen-containing compound not corresponding to the formula (1) is any one or more selected from imidazole, triethylamine, and tripropylamine.
[12] The method for producing a capacitor according to any one of [9] to [11], wherein in the formula (1), at least one of R 1 , R 2 , and R 3 is an amino group. .
[13] The method for producing a capacitor according to any one of [9] to [12], wherein the π-conjugated conductive polymer is poly (3,4-ethylenedioxythiophene).
[14] The method for producing a capacitor according to any one of [9] to [13], wherein the polyanion is polystyrene sulfonic acid.

本発明のキャパシタの等価直列抵抗は従来よりも小さく、電子機器の高性能化に資する。
本発明のキャパシタの製造方法によれば、等価直列抵抗が小さいキャパシタを容易に製造することができる。
The equivalent series resistance of the capacitor of the present invention is smaller than that of the conventional one, which contributes to high performance of electronic equipment.
According to the method for manufacturing a capacitor of the present invention, a capacitor having a small equivalent series resistance can be easily manufactured.

本発明のキャパシタの一実施形態を示す断面図である。It is sectional drawing which shows one Embodiment of the capacitor of this invention.

《キャパシタ》
本発明のキャパシタの一実施形態について説明する。図1に示すように、本実施形態のキャパシタ10は、弁金属の多孔質体からなる陽極11と、弁金属の酸化物からなる誘電体層12と、誘電体層12の表面に形成された固体電解質層14と、最も表側に設けられた陰極13とを具備する。
<Capacitor>
One embodiment of the capacitor of the present invention will be described. As shown in FIG. 1, the capacitor 10 of this embodiment is formed on the surface of the anode 11 made of a porous body of the valve metal, the dielectric layer 12 made of the oxide of the valve metal, and the dielectric layer 12. A solid electrolyte layer 14 and a cathode 13 provided on the most front side are provided.

陽極11を構成する弁金属としては、例えば、アルミニウム、タンタル、ニオブ、チタン、ハフニウム、ジルコニウム、亜鉛、タングステン、ビスマス、アンチモンなどが挙げられる。これらのうち、アルミニウム、タンタル、ニオブが好適である。
陽極11の具体例としては、アルミニウム箔をエッチングして表面積を増加させた後、その表面を酸化処理したものや、タンタル粒子やニオブ粒子の焼結体表面を酸化処理してペレットにしたものが挙げられる。このように処理されたものは表面に凹凸が形成された多孔質体となる。
Examples of the valve metal constituting the anode 11 include aluminum, tantalum, niobium, titanium, hafnium, zirconium, zinc, tungsten, bismuth, and antimony. Of these, aluminum, tantalum, and niobium are preferable.
Specific examples of the anode 11 include those obtained by etching an aluminum foil to increase the surface area and then oxidizing the surface, or oxidizing the surface of a sintered body of tantalum particles and niobium particles into pellets. Can be mentioned. What was processed in this way becomes a porous body having irregularities formed on the surface.

本実施形態における誘電体層12は、陽極11の表面が酸化されて形成された層であり、例えば、アジピン酸アンモニウム水溶液などの電解液中にて、金属体の陽極11の表面を陽極酸化することで形成されたものである。よって、図1に示すように、陽極11と同様に誘電体層12にも凹凸が形成されている。   The dielectric layer 12 in the present embodiment is a layer formed by oxidizing the surface of the anode 11. For example, the surface of the anode 11 of the metal body is anodized in an electrolytic solution such as an aqueous solution of ammonium adipate. It is formed by. Therefore, as shown in FIG. 1, the dielectric layer 12 is also uneven as in the anode 11.

本実施形態における陰極13としては、導電性ペーストから形成した導電層やアルミニウム箔など、導電物質製の金属層を使用することができる。   As the cathode 13 in the present embodiment, a metal layer made of a conductive material such as a conductive layer formed from a conductive paste or an aluminum foil can be used.

本実施形態における固体電解質層14は、第一の固体電解質層と、第二の固体電解質層とがこの順で誘電体層12の表面に積層された構造を有する。第一の固体電解質層は、誘電体層12の表面の少なくとも一部を覆っており、誘電体層12の表面の全部を覆っていてもよい。第二の固体電解質層は、第一の固体電解質層の少なくとも一部を覆っており、第一の固体電解質層の全部を覆っていてもよい。第一の固体電解質層が誘電体層12の一部を覆い、第二の固体電解質層が第一の固体電解質層を覆う構成において、第二の固体電解質層は、第一の固体電解質層に覆われていない誘電体層12の残部も覆うことが好ましい。
本実施形態では第一の固体電解質層と第二の固体電解質層との境界が明確に分かれている場合について説明するが、その境界が明確に分かれていなくても構わない。
The solid electrolyte layer 14 in the present embodiment has a structure in which a first solid electrolyte layer and a second solid electrolyte layer are laminated on the surface of the dielectric layer 12 in this order. The first solid electrolyte layer covers at least a part of the surface of the dielectric layer 12 and may cover the entire surface of the dielectric layer 12. The second solid electrolyte layer covers at least a part of the first solid electrolyte layer, and may cover the entire first solid electrolyte layer. In the configuration in which the first solid electrolyte layer covers a part of the dielectric layer 12 and the second solid electrolyte layer covers the first solid electrolyte layer, the second solid electrolyte layer is formed on the first solid electrolyte layer. It is preferable to cover the remainder of the dielectric layer 12 that is not covered.
In the present embodiment, a case where the boundary between the first solid electrolyte layer and the second solid electrolyte layer is clearly separated will be described, but the boundary may not be clearly separated.

固体電解質層14の厚さは、一定でもよいし、一定でなくてもよく、例えば、1μm以上100μm以下の範囲内の厚さが挙げられる。
第一の固体電解質層の厚さt1と第二の固体電解質層の厚さt2の相対比(t1/t2)は、特に限定されず、例えば、10/1〜1/10が挙げられる。
The thickness of the solid electrolyte layer 14 may or may not be constant, and examples thereof include a thickness in the range of 1 μm to 100 μm.
The relative ratio (t1 / t2) between the thickness t1 of the first solid electrolyte layer and the thickness t2 of the second solid electrolyte layer is not particularly limited, and examples thereof include 10/1 to 1/10.

第一の固体電解質層は、後述する式(1)で表されるアジン化合物を含有している。
第二の固体電解質層は、後で詳述するπ共役系導電性高分子及びポリアニオンを含む導電性複合体を含有している。
第一の固体電解質層は、前記導電性複合体を含有してもよいし、含有しなくてもよい。
第二の固体電解質層は、後述する式(1)で表されるアジン化合物を含有してもよいし、含有しなくてもよい。
The first solid electrolyte layer contains an azine compound represented by the following formula (1).
The second solid electrolyte layer contains a conductive complex including a π-conjugated conductive polymer and a polyanion described in detail later.
The first solid electrolyte layer may or may not contain the conductive composite.
The second solid electrolyte layer may or may not contain an azine compound represented by the formula (1) described later.

本実施形態の固体電解質層は、下記式(1)で表されるアジン化合物を含有している。   The solid electrolyte layer of the present embodiment contains an azine compound represented by the following formula (1).

Figure 2018085420
[式(1)中、X,X,Xは各々独立してCH又はNであり、R,R,Rは各々独立して水素原子又は任意の置換基であり、X,X,Xのうち少なくとも何れか1つはNであり、R,R,Rのうち少なくとも何れか1つは窒素を有する置換基である。]
Figure 2018085420
[In the formula (1), X 1 , X 2 and X 3 are each independently CH or N, R 1 , R 2 and R 3 are each independently a hydrogen atom or an arbitrary substituent; At least one of 1 , X 2 and X 3 is N, and at least one of R 1 , R 2 and R 3 is a nitrogen-containing substituent. ]

前記X,X,Xのうち、何れか1つがNであってもよいし、何れか2つがNであってもよいし、3つ全てがNであってもよい。 Any one of X 1 , X 2 , and X 3 may be N, any two may be N, or all three may be N.

前記R,R,Rの何れかが任意の置換基である場合、その任意の置換基としては、例えば、アルキル基(例えば、メチル基、エチル基、プロピル基、ブチル基等)、アルケニル基(例えば、ビニル基、アリル基等)、アルコキシ基(例えば、メトキシ基、エトキシ基、プロポキシ基、ブトキシ基、等)、アリール基(例えば、フェニル基等)等が挙げられる。これらの置換基は、さらに別の置換基(例えば、アリルオキシ基、(メタ)アクリロイルオキシ基、カルボキシ基、ヒドロキシ基、メルカプト基、エポキシ基、アミノ基、トリアルコキシシリル基等)を有してもよい。 When any of R 1 , R 2 and R 3 is an optional substituent, examples of the optional substituent include an alkyl group (for example, a methyl group, an ethyl group, a propyl group, a butyl group), Examples include an alkenyl group (for example, vinyl group, allyl group, etc.), an alkoxy group (for example, methoxy group, ethoxy group, propoxy group, butoxy group, etc.), an aryl group (for example, phenyl group, etc.) and the like. These substituents may have another substituent (for example, allyloxy group, (meth) acryloyloxy group, carboxy group, hydroxy group, mercapto group, epoxy group, amino group, trialkoxysilyl group, etc.). Good.

前記R,R,Rの何れかが窒素を有する置換基である場合、その置換基はアミノ基であることが好ましい。前記アミノ基を構成する水素原子は、さらに別の置換基によって置換されていてもよい。前記別の置換基としては、例えば、メチル基、エチル基、プロピル基、ブチル基等のアルキル基;アリル基などのアルケニル基;メトキシメチル基、エトキシメチル基、メトキシエチル基、エトキシエチル基等のアルコキシアルキル基;(メタ)アクリロイルオキシ基、カルボキシ基、ヒドロキシ基、エポキシ基、アミノ基、トリアルコキシシリル基等が挙げられる。 When any of R 1 , R 2 , and R 3 is a nitrogen-containing substituent, the substituent is preferably an amino group. The hydrogen atom constituting the amino group may be further substituted with another substituent. Examples of the other substituent include an alkyl group such as a methyl group, an ethyl group, a propyl group, and a butyl group; an alkenyl group such as an allyl group; a methoxymethyl group, an ethoxymethyl group, a methoxyethyl group, and an ethoxyethyl group. An alkoxyalkyl group; a (meth) acryloyloxy group, a carboxy group, a hydroxy group, an epoxy group, an amino group, a trialkoxysilyl group, and the like.

前記式(1)で表されるアジン化合物の好適な具体例として、例えば、メラミン、アセトグアナミン、2,4,6−[トリス(ビスメトキシメチル) アミノ]−1,3,5−トリアジン、2,4,6−トリアミノピリミジン、2−アミノピリミジン、p−アミノピリジン(4−アミノピリジン)、N,N−ジメチル−4−アミノピリジン(DMAP)等が挙げられる。これらのアジン化合物が固体電解質層に含有されていると、キャパシタの等価直列抵抗がより低下し易くなるので好ましい。   Preferable specific examples of the azine compound represented by the formula (1) include, for example, melamine, acetoguanamine, 2,4,6- [tris (bismethoxymethyl) amino] -1,3,5-triazine, 2 , 4,6-triaminopyrimidine, 2-aminopyrimidine, p-aminopyridine (4-aminopyridine), N, N-dimethyl-4-aminopyridine (DMAP) and the like. It is preferable that these azine compounds are contained in the solid electrolyte layer because the equivalent series resistance of the capacitor is more likely to decrease.

第一の固体電解質層の総質量に対するアジン化合物の含有量は、80質量%以上100質量%以下が好ましく、90質量%以上100質量%以下がより好ましく、95質量%以上100質量%以下がさらに好ましい。上記の範囲であると、キャパシタの等価直列抵抗がより低下し易くなるので好ましい。   The content of the azine compound with respect to the total mass of the first solid electrolyte layer is preferably 80% by mass or more and 100% by mass or less, more preferably 90% by mass or more and 100% by mass or less, and further more preferably 95% by mass or more and 100% by mass or less. preferable. The above range is preferable because the equivalent series resistance of the capacitor is more likely to decrease.

次に、第二の固体電解質層に含有されるπ共役系導電性高分子及びポリアニオンを含む導電性複合体について説明する。
π共役系導電性高分子としては、主鎖がπ共役系で構成されている有機高分子であれば特に制限されず、例えば、ポリピロール系導電性高分子、ポリチオフェン系導電性高分子、ポリアセチレン系導電性高分子、ポリフェニレン系導電性高分子、ポリフェニレンビニレン系導電性高分子、ポリアニリン系導電性高分子、ポリアセン系導電性高分子、ポリチオフェンビニレン系導電性高分子、及びこれらの共重合体等が挙げられる。空気中での安定性の点からは、ポリピロール系導電性高分子、ポリチオフェン類及びポリアニリン系導電性高分子が好ましく、ポリチオフェン系導電性高分子がより好ましい。
Next, a conductive composite containing a π-conjugated conductive polymer and a polyanion contained in the second solid electrolyte layer will be described.
The π-conjugated conductive polymer is not particularly limited as long as the main chain is an organic polymer composed of a π-conjugated system. For example, a polypyrrole-based conductive polymer, a polythiophene-based conductive polymer, a polyacetylene-based polymer Conductive polymers, polyphenylene conductive polymers, polyphenylene vinylene conductive polymers, polyaniline conductive polymers, polyacene conductive polymers, polythiophene vinylene conductive polymers, and copolymers thereof Can be mentioned. From the viewpoint of stability in air, polypyrrole conductive polymers, polythiophenes and polyaniline conductive polymers are preferable, and polythiophene conductive polymers are more preferable.

ポリチオフェン系導電性高分子としては、例えば、ポリチオフェン、ポリ(3−メチルチオフェン)、ポリ(3−エチルチオフェン)、ポリ(3−プロピルチオフェン)、ポリ(3−ブチルチオフェン)、ポリ(3−ヘキシルチオフェン)、ポリ(3−ヘプチルチオフェン)、ポリ(3−オクチルチオフェン)、ポリ(3−デシルチオフェン)、ポリ(3−ドデシルチオフェン)、ポリ(3−オクタデシルチオフェン)、ポリ(3−ブロモチオフェン)、ポリ(3−クロロチオフェン)、ポリ(3−ヨードチオフェン)、ポリ(3−シアノチオフェン)、ポリ(3−フェニルチオフェン)、ポリ(3,4−ジメチルチオフェン)、ポリ(3,4−ジブチルチオフェン)、ポリ(3−ヒドロキシチオフェン)、ポリ(3−メトキシチオフェン)、ポリ(3−エトキシチオフェン)、ポリ(3−ブトキシチオフェン)、ポリ(3−ヘキシルオキシチオフェン)、ポリ(3−ヘプチルオキシチオフェン)、ポリ(3−オクチルオキシチオフェン)、ポリ(3−デシルオキシチオフェン)、ポリ(3−ドデシルオキシチオフェン)、ポリ(3−オクタデシルオキシチオフェン)、ポリ(3,4−ジヒドロキシチオフェン)、ポリ(3,4−ジメトキシチオフェン)、ポリ(3,4−ジエトキシチオフェン)、ポリ(3,4−ジプロポキシチオフェン)、ポリ(3,4−ジブトキシチオフェン)、ポリ(3,4−ジヘキシルオキシチオフェン)、ポリ(3,4−ジヘプチルオキシチオフェン)、ポリ(3,4−ジオクチルオキシチオフェン)、ポリ(3,4−ジデシルオキシチオフェン)、ポリ(3,4−ジドデシルオキシチオフェン)、ポリ(3,4−エチレンジオキシチオフェン)、ポリ(3,4−プロピレンジオキシチオフェン)、ポリ(3,4−ブチレンジオキシチオフェン)、ポリ(3−メチル−4−メトキシチオフェン)、ポリ(3−メチル−4−エトキシチオフェン)、ポリ(3−カルボキシチオフェン)、ポリ(3−メチル−4−カルボキシチオフェン)、ポリ(3−メチル−4−カルボキシエチルチオフェン)、ポリ(3−メチル−4−カルボキシブチルチオフェン)が挙げられる。   Examples of the polythiophene-based conductive polymer include polythiophene, poly (3-methylthiophene), poly (3-ethylthiophene), poly (3-propylthiophene), poly (3-butylthiophene), and poly (3-hexyl). Thiophene), poly (3-heptylthiophene), poly (3-octylthiophene), poly (3-decylthiophene), poly (3-dodecylthiophene), poly (3-octadecylthiophene), poly (3-bromothiophene) , Poly (3-chlorothiophene), poly (3-iodothiophene), poly (3-cyanothiophene), poly (3-phenylthiophene), poly (3,4-dimethylthiophene), poly (3,4-dibutyl) Thiophene), poly (3-hydroxythiophene), poly (3-methoxythiophene) Poly (3-ethoxythiophene), poly (3-butoxythiophene), poly (3-hexyloxythiophene), poly (3-heptyloxythiophene), poly (3-octyloxythiophene), poly (3-decyloxythiophene) ), Poly (3-dodecyloxythiophene), poly (3-octadecyloxythiophene), poly (3,4-dihydroxythiophene), poly (3,4-dimethoxythiophene), poly (3,4-diethoxythiophene) , Poly (3,4-dipropoxythiophene), poly (3,4-dibutoxythiophene), poly (3,4-dihexyloxythiophene), poly (3,4-diheptyloxythiophene), poly (3,4 4-dioctyloxythiophene), poly (3,4-didecyloxythiophene), poly (3,4-didodecyloxythiophene), poly (3,4-ethylenedioxythiophene), poly (3,4-propylenedioxythiophene), poly (3,4-butylenedioxythiophene), poly (3 -Methyl-4-methoxythiophene), poly (3-methyl-4-ethoxythiophene), poly (3-carboxythiophene), poly (3-methyl-4-carboxythiophene), poly (3-methyl-4-carboxy) Ethylthiophene) and poly (3-methyl-4-carboxybutylthiophene).

ポリピロール系導電性高分子としては、例えば、ポリピロール、ポリ(N−メチルピロール)、ポリ(3−メチルピロール)、ポリ(3−エチルピロール)、ポリ(3−n−プロピルピロール)、ポリ(3−ブチルピロール)、ポリ(3−オクチルピロール)、ポリ(3−デシルピロール)、ポリ(3−ドデシルピロール)、ポリ(3,4−ジメチルピロール)、ポリ(3,4−ジブチルピロール)、ポリ(3−カルボキシピロール)、ポリ(3−メチル−4−カルボキシピロール)、ポリ(3−メチル−4−カルボキシエチルピロール)、ポリ(3−メチル−4−カルボキシブチルピロール)、ポリ(3−ヒドロキシピロール)、ポリ(3−メトキシピロール)、ポリ(3−エトキシピロール)、ポリ(3−ブトキシピロール)、ポリ(3−ヘキシルオキシピロール)、ポリ(3−メチル−4−ヘキシルオキシピロール)が挙げられる。   Examples of the polypyrrole-based conductive polymer include polypyrrole, poly (N-methylpyrrole), poly (3-methylpyrrole), poly (3-ethylpyrrole), poly (3-n-propylpyrrole), and poly (3 -Butylpyrrole), poly (3-octylpyrrole), poly (3-decylpyrrole), poly (3-dodecylpyrrole), poly (3,4-dimethylpyrrole), poly (3,4-dibutylpyrrole), poly (3-carboxypyrrole), poly (3-methyl-4-carboxypyrrole), poly (3-methyl-4-carboxyethylpyrrole), poly (3-methyl-4-carboxybutylpyrrole), poly (3-hydroxy Pyrrole), poly (3-methoxypyrrole), poly (3-ethoxypyrrole), poly (3-butoxypyrrole), poly (3 Hexyloxy pyrrole), poly (3-methyl-4-hexyloxy-pyrrole) and the like.

ポリアニリン系導電性高分子としては、例えば、ポリアニリン、ポリ(2−メチルアニリン)、ポリ(3−イソブチルアニリン)、ポリ(2−アニリンスルホン酸)、ポリ(3−アニリンスルホン酸)が挙げられる。
以上で例示したπ共役系導電性高分子の中でも、導電性、耐熱性の点から、ポリ(3,4−エチレンジオキシチオフェン)が特に好ましい。
π共役系導電性高分子は1種を単独で使用してもよいし、2種以上を併用してもよい。
Examples of the polyaniline-based conductive polymer include polyaniline, poly (2-methylaniline), poly (3-isobutylaniline), poly (2-aniline sulfonic acid), and poly (3-aniline sulfonic acid).
Among the π-conjugated conductive polymers exemplified above, poly (3,4-ethylenedioxythiophene) is particularly preferable from the viewpoint of conductivity and heat resistance.
One kind of π-conjugated conductive polymer may be used alone, or two or more kinds may be used in combination.

ポリアニオンとは、アニオン基を有するモノマー単位を、分子内に2つ以上有する重合体である。このポリアニオンのアニオン基は、π共役系導電性高分子に対するドーパントとして機能して、π共役系導電性高分子の導電性を向上させることができる。
ポリアニオンのアニオン基は、スルホ基またはカルボキシ基であることが好ましい。
ポリアニオンの具体例としては、ポリスチレンスルホン酸、ポリビニルスルホン酸、ポリアリルスルホン酸、ポリアクリルスルホン酸、ポリメタクリルスルホン酸、ポリ(2−アクリルアミド−2−メチルプロパンスルホン酸)、ポリイソプレンスルホン酸、ポリスルホエチルメタクリレート、ポリ(4−スルホブチルメタクリレート)、ポリメタクリルオキシベンゼンスルホン酸等のスルホン酸基を有する高分子や、ポリビニルカルボン酸、ポリスチレンカルボン酸、ポリアリルカルボン酸、ポリアクリルカルボン酸、ポリメタクリルカルボン酸、ポリ(2−アクリルアミド−2−メチルプロパンカルボン酸)、ポリイソプレンカルボン酸、ポリアクリル酸等のカルボン酸基を有する高分子が挙げられる。これらの単独重合体であってもよいし、2種以上の共重合体であってもよい。
これらのポリアニオンのなかでも、導電性をより高くできることから、スルホン酸基を有する高分子が好ましく、ポリスチレンスルホン酸がより好ましい。
ポリアニオンは1種を単独で使用してもよいし、2種以上を併用してもよい。
ポリアニオンの質量平均分子量は2万以上100万以下であることが好ましく、10万以上50万以下であることがより好ましい。
本明細書における質量平均分子量は、ゲルパーミエーションクロマトグラフィで測定し、標準物質をポリスチレンとして求めた値である。
The polyanion is a polymer having two or more monomer units having an anion group in the molecule. The anion group of the polyanion functions as a dopant for the π-conjugated conductive polymer, and can improve the conductivity of the π-conjugated conductive polymer.
The anion group of the polyanion is preferably a sulfo group or a carboxy group.
Specific examples of polyanions include polystyrene sulfonic acid, polyvinyl sulfonic acid, polyallyl sulfonic acid, polyacryl sulfonic acid, polymethacryl sulfonic acid, poly (2-acrylamido-2-methylpropane sulfonic acid), polyisoprene sulfonic acid, poly Polymers having a sulfonic acid group such as sulfoethyl methacrylate, poly (4-sulfobutyl methacrylate), polymethacryloxybenzene sulfonic acid, polyvinyl carboxylic acid, polystyrene carboxylic acid, polyallyl carboxylic acid, polyacryl carboxylic acid, polymethacrylic acid Examples thereof include polymers having a carboxylic acid group such as carboxylic acid, poly (2-acrylamido-2-methylpropanecarboxylic acid), polyisoprene carboxylic acid, and polyacrylic acid. These homopolymers may be sufficient and 2 or more types of copolymers may be sufficient.
Among these polyanions, a polymer having a sulfonic acid group is preferable and polystyrene sulfonic acid is more preferable because conductivity can be further increased.
A polyanion may be used individually by 1 type, and may use 2 or more types together.
The mass average molecular weight of the polyanion is preferably 20,000 or more and 1,000,000 or less, and more preferably 100,000 or more and 500,000 or less.
The mass average molecular weight in the present specification is a value obtained by measuring with gel permeation chromatography and obtaining the standard substance as polystyrene.

導電性複合体中の、ポリアニオンの含有割合は、π共役系導電性高分子100質量部に対して1質量部以上1000質量部以下の範囲であることが好ましく、10質量部以上700質量部以下の範囲であることがより好ましく、100質量部以上500質量部以下の範囲であることがさらに好ましい。ポリアニオンの含有割合が前記下限値未満であると、π共役系導電性高分子へのドーピング効果が弱くなる傾向にあり、導電性が不足することがあり、また、導電性高分子分散液における導電性複合体の分散性が低くなる。一方、ポリアニオンの含有量が前記上限値を超えると、π共役系導電性高分子の含有量が少なくなり、やはり充分な導電性が得られにくい。   The content ratio of the polyanion in the conductive composite is preferably in the range of 1 part by mass to 1000 parts by mass with respect to 100 parts by mass of the π-conjugated conductive polymer, and 10 parts by mass to 700 parts by mass. It is more preferable that it is the range of 100 mass parts or more and 500 mass parts or less. If the polyanion content is less than the lower limit, the doping effect on the π-conjugated conductive polymer tends to be weak, the conductivity may be insufficient, and the conductivity in the conductive polymer dispersion may be insufficient. The dispersibility of the sex complex decreases. On the other hand, when the content of the polyanion exceeds the upper limit, the content of the π-conjugated conductive polymer is decreased, and it is difficult to obtain sufficient conductivity.

ポリアニオンがπ共役系導電性高分子に配位してドープすることによって導電性複合体が形成される。
ただし、本実施形態におけるポリアニオンにおいては、全てのアニオン基がπ共役系導電性高分子にドープすることはなく、ドープに寄与しない余剰のアニオン基を有するようになっている。
A conductive complex is formed by coordinating and doping a polyanion with a π-conjugated conductive polymer.
However, in the polyanion in this embodiment, not all anion groups are doped into the π-conjugated conductive polymer, but have an excess anion group that does not contribute to doping.

第二の固体電解質層の総質量に対する導電性複合体の含有量は、80質量%以上100質量%以下が好ましく、90質量%以上100質量%以下がより好ましく、95質量%以上100質量%以下がさらに好ましい。上記の範囲であると、キャパシタの等価直列抵抗がより低下し易くなるので好ましい。   The content of the conductive composite with respect to the total mass of the second solid electrolyte layer is preferably 80% by mass or more and 100% by mass or less, more preferably 90% by mass or more and 100% by mass or less, and 95% by mass or more and 100% by mass or less. Is more preferable. The above range is preferable because the equivalent series resistance of the capacitor is more likely to decrease.

前記固体電解質層の第一の固体電解質層及び第二の固体電解質層のうち少なくとも一方には、前記式(1)に該当しない含窒素化合物の1種以上がさらに含有されていてもよい。この含窒素化合物が固体電解質層に含まれることによって、キャパシタの等価直列抵抗をさらに低減できることがある。   At least one of the first solid electrolyte layer and the second solid electrolyte layer of the solid electrolyte layer may further contain one or more nitrogen-containing compounds not corresponding to the formula (1). By including this nitrogen-containing compound in the solid electrolyte layer, the equivalent series resistance of the capacitor may be further reduced.

前記含窒素化合物として、以下のアミン化合物及び窒素含有芳香族性化合物を例示できる。これらのアミン化合物及び窒素含有芳香族性化合物の少なくともどちらか一方が固体電解質層に含まれると、キャパシタの等価直列抵抗をさらに低減できることがある。
アミン化合物は、アミノ基を有する化合物であり、アミノ基が、ポリアニオンのアニオン基と反応する。
アミン化合物としては、1級アミン、2級アミン、3級アミン、4級アンモニウム塩のいずれであってもよい。また、アミン化合物は1種を単独で使用してもよいし、2種以上を併用してもよい。
アミン化合物は、炭素数2以上12以下の直鎖、もしくは分岐鎖のアルキル基、炭素数6以上12以下のアリール基、炭素数7以上12以下のアラルキル基、炭素数2以上12以下のアルキレン基、炭素数6以上12以下のアリーレン基、炭素数7以上12以下のアラルキレン基、及び炭素数2以上12以下のオキシアルキレン基から選択される置換基を有していてもよい。
具体的な1級アミンとしては、例えば、アニリン、トルイジン、ベンジルアミン、エタノールアミン等が挙げられる。
具体的な2級アミンとしては、例えば、ジエタノールアミン、ジメチルアミン、ジエチルアミン、ジプロピルアミン、ジフェニルアミン、ジベンジルアミン、ジナフチルアミン等が挙げられる。
具体的な3級アミンとしては、例えば、トリエタノールアミン、トリメチルアミン、トリエチルアミン、トリプロピルアミン、トリブチルアミン、トリオクチルアミン、トリフェニルアミン、トリベンジルアミン、トリナフチルアミン等が挙げられる。
具体的な4級アンモニウム塩としては、例えば、テトラメチルアンモニウム塩、テトラエチルアンモニウム塩、テトラプロピルアンモニウム塩、テトラフェニルアンモニウム塩、テトラベンジルアンモニウム塩、テトラナフチルアンモニウム塩等が挙げられる。アンモニウムの対となる陰イオンとしてはヒドロキシドイオンが挙げられる。
これらアミン化合物のうち、3級アミンが好ましく、トリエチルアミン、トリプロピルアミンがより好ましい。
窒素含有芳香族性化合物としては、例えば、アニリン、ベンジルアミン、ピロール、イミダゾール、2−メチルイミダゾール、2−プロピルイミダゾール、N−メチルイミダゾール、N−プロピルイミダゾール、N−ブチルイミダゾール、1−(2−ヒドロキシエチル)イミダゾール、2−エチル−4−メチルイミダゾール、1,2−ジメチルイミダゾール、1−ベンジル−2−メチルイミダゾール、1−シアノエチル−2−メチルイミダゾール、1−シアノエチル−2−エチル−4−メチルイミダゾール、2−フェニル−4,5−ジヒドロキシメチルイミダゾール、1−アセチルイミダゾール、2−アミノベンズイミダゾール、2−アミノ−1−メチルベンズイミダゾール、2−ヒドロキシベンズイミダゾール、2−(2−ピリジル)ベンズイミダゾール、ピリジン等が挙げられる。
これら窒素含有芳香族性化合物のうち、イミダゾールがより好ましい。
Examples of the nitrogen-containing compound include the following amine compounds and nitrogen-containing aromatic compounds. When at least one of these amine compounds and nitrogen-containing aromatic compounds is contained in the solid electrolyte layer, the equivalent series resistance of the capacitor may be further reduced.
The amine compound is a compound having an amino group, and the amino group reacts with the anion group of the polyanion.
The amine compound may be any of primary amine, secondary amine, tertiary amine, and quaternary ammonium salt. Moreover, an amine compound may be used individually by 1 type, and may use 2 or more types together.
The amine compound is a linear or branched alkyl group having 2 to 12 carbon atoms, an aryl group having 6 to 12 carbon atoms, an aralkyl group having 7 to 12 carbon atoms, or an alkylene group having 2 to 12 carbon atoms. And a substituent selected from an arylene group having 6 to 12 carbon atoms, an aralkylene group having 7 to 12 carbon atoms, and an oxyalkylene group having 2 to 12 carbon atoms.
Specific examples of the primary amine include aniline, toluidine, benzylamine, and ethanolamine.
Specific examples of the secondary amine include diethanolamine, dimethylamine, diethylamine, dipropylamine, diphenylamine, dibenzylamine, and dinaphthylamine.
Specific examples of the tertiary amine include triethanolamine, trimethylamine, triethylamine, tripropylamine, tributylamine, trioctylamine, triphenylamine, tribenzylamine, and trinaphthylamine.
Specific examples of the quaternary ammonium salt include tetramethylammonium salt, tetraethylammonium salt, tetrapropylammonium salt, tetraphenylammonium salt, tetrabenzylammonium salt, tetranaphthylammonium salt and the like. A hydroxide ion is mentioned as an anion which becomes a pair of ammonium.
Of these amine compounds, tertiary amines are preferred, and triethylamine and tripropylamine are more preferred.
Examples of the nitrogen-containing aromatic compound include aniline, benzylamine, pyrrole, imidazole, 2-methylimidazole, 2-propylimidazole, N-methylimidazole, N-propylimidazole, N-butylimidazole, 1- (2- Hydroxyethyl) imidazole, 2-ethyl-4-methylimidazole, 1,2-dimethylimidazole, 1-benzyl-2-methylimidazole, 1-cyanoethyl-2-methylimidazole, 1-cyanoethyl-2-ethyl-4-methyl Imidazole, 2-phenyl-4,5-dihydroxymethylimidazole, 1-acetylimidazole, 2-aminobenzimidazole, 2-amino-1-methylbenzimidazole, 2-hydroxybenzimidazole, 2- (2-pyridyl) ben Imidazole, pyridine, and the like.
Of these nitrogen-containing aromatic compounds, imidazole is more preferred.

前記固体電解質層には、電解液用溶媒中に電解質を溶解させた電解液が含まれてもよい。電解液の電気伝導度は高いほど好ましい。
電解液用溶媒としては、例えば、エチレングリコール、ジエチレングリコール、プロピレングリコール、1,4−ブタンジオール、グリセリン等のアルコール系溶媒、γ−ブチロラクトン、γ−バレロラクトン、δ−バレロラクトン等のラクトン系溶媒、N−メチルホルムアミド、N,N−ジメチルホルムアミド、N−メチルアセトアミド、N−メチルピロリジノン等のアミド系溶媒、アセトニトリル、3−メトキシプロピオニトリル等のニトリル系溶媒、水等が挙げられる。
電解質としては、例えば、アジピン酸、グルタル酸、コハク酸、安息香酸、イソフタル酸、フタル酸、テレフタル酸、マレイン酸、トルイル酸、エナント酸、マロン酸、蟻酸、1,6−デカンジカルボン酸、5,6−デカンジカルボン酸等のデカンジカルボン酸、1,7−オクタンジカルボン酸等のオクタンジカルボン酸、アゼライン酸、セバシン酸等の有機酸;あるいは、硼酸、硼酸と多価アルコールより得られる硼酸の多価アルコール錯化合物;リン酸、炭酸、ケイ酸等の無機酸などをアニオン成分とし、1級アミン(メチルアミン、エチルアミン、プロピルアミン、ブチルアミン、エチレンジアミン等)、2級アミン(ジメチルアミン、ジエチルアミン、ジプロピルアミン、メチルエチルアミン、ジフェニルアミン等)、3級アミン(トリメチルアミン、トリエチルアミン、トリプロピルアミン、トリフェニルアミン、1,8−ジアザビシクロ(5,4,0)−ウンデセン−7等)、テトラアルキルアンモニウム(テトラメチルアンモニウム、テトラエチルアンモニウム、テトラプロピルアンモニウム、テトラブチルアンモニウム、メチルトリエチルアンモニウム、ジメチルジエチルアンモニウム等)などをカチオン成分とした電解質;等が挙げられる。
The solid electrolyte layer may include an electrolytic solution in which an electrolyte is dissolved in a solvent for the electrolytic solution. The higher the electric conductivity of the electrolytic solution, the better.
Examples of the electrolyte solution solvent include alcohol solvents such as ethylene glycol, diethylene glycol, propylene glycol, 1,4-butanediol, and glycerin; lactone solvents such as γ-butyrolactone, γ-valerolactone, and δ-valerolactone; Examples thereof include amide solvents such as N-methylformamide, N, N-dimethylformamide, N-methylacetamide and N-methylpyrrolidinone, nitrile solvents such as acetonitrile and 3-methoxypropionitrile, water and the like.
Examples of the electrolyte include adipic acid, glutaric acid, succinic acid, benzoic acid, isophthalic acid, phthalic acid, terephthalic acid, maleic acid, toluic acid, enanthic acid, malonic acid, formic acid, 1,6-decanedicarboxylic acid, 5 Decane dicarboxylic acid such as 1,6-decanedicarboxylic acid, octane dicarboxylic acid such as 1,7-octane dicarboxylic acid, organic acid such as azelaic acid and sebacic acid; or boric acid, a large amount of boric acid obtained from boric acid and polyhydric alcohol Monohydric alcohol complex compounds: primary acids (methylamine, ethylamine, propylamine, butylamine, ethylenediamine, etc.), secondary amines (dimethylamine, diethylamine, diamine) containing inorganic acids such as phosphoric acid, carbonic acid, and silicic acid as anion components Propylamine, methylethylamine, diphenylamine, etc.), tertiary amine ( Limethylamine, triethylamine, tripropylamine, triphenylamine, 1,8-diazabicyclo (5,4,0) -undecene-7, etc.), tetraalkylammonium (tetramethylammonium, tetraethylammonium, tetrapropylammonium, tetrabutylammonium, Electrolytes having a cation component such as methyltriethylammonium and dimethyldiethylammonium).

<作用効果>
本発明のキャパシタの固体電解質層に前記式(1)で表されるアジン化合物が含有されることによって、静電容量を低下させることなく、キャパシタの等価直列抵抗を従来よりも低減することができる。このメカニズムは未解明であるが、前記アジン化合物が固体電解質層の導電性を向上させることによって、その等価直列抵抗が小さくなったと推測される。
<Effect>
By containing the azine compound represented by the formula (1) in the solid electrolyte layer of the capacitor of the present invention, the equivalent series resistance of the capacitor can be reduced more than before without reducing the capacitance. . Although this mechanism is not yet elucidated, it is presumed that the equivalent series resistance is reduced by the azine compound improving the conductivity of the solid electrolyte layer.

《キャパシタの製造方法》
本発明にかかるキャパシタは、弁金属の多孔質体からなる陽極の表面を酸化して誘電体層を形成する工程(誘電体形成工程)と、前記誘電体層に対向する位置に陰極を配置する工程(陰極形成工程)と、前記誘電体層の表面の少なくとも一部に、前記式(1)で表されるアジン化合物を含む溶液を塗布し、乾燥させて、第一の固体電解質層を形成する工程(第一の固体電解質層形成工程)と、前記第一の固体電解質層の表面の少なくとも一部に、π共役系導電性高分子及びポリアニオンを含む導電性複合体が分散された導電性高分子分散液を塗布し、乾燥させて、第二の固体電解質層を形成する工程(第二の固体電解質層形成工程)と、によって製造することができる。
<< Capacitor Manufacturing Method >>
The capacitor according to the present invention includes a step of forming a dielectric layer by oxidizing the surface of the anode made of a porous body of valve metal (dielectric formation step), and disposing a cathode at a position facing the dielectric layer. Step (cathode formation step) and applying a solution containing the azine compound represented by the formula (1) to at least a part of the surface of the dielectric layer and drying to form a first solid electrolyte layer A first solid electrolyte layer forming step, and a conductivity in which a conductive complex containing a π-conjugated conductive polymer and a polyanion is dispersed on at least a part of the surface of the first solid electrolyte layer The polymer dispersion can be applied and dried to form a second solid electrolyte layer (second solid electrolyte layer forming step).

誘電体層形成工程は、弁金属の多孔質体からなる陽極11の表面を酸化して誘電体層12を形成する工程である。
誘電体層12を形成する方法としては、例えば、アジピン酸アンモニウム水溶液、ホウ酸アンモニウム水溶液、リン酸アンモニウム水溶液などの化成処理用電解液中にて、陽極11の表面を陽極酸化する方法が挙げられる。
The dielectric layer forming step is a step of forming the dielectric layer 12 by oxidizing the surface of the anode 11 made of a porous body of valve metal.
Examples of the method for forming the dielectric layer 12 include a method in which the surface of the anode 11 is anodized in an electrolytic solution for chemical conversion treatment such as an aqueous solution of ammonium adipate, an aqueous solution of ammonium borate, or an aqueous solution of ammonium phosphate. .

陰極形成工程は、誘電体層12に対向する位置に陰極13を配置する工程である。
陰極13を配置する方法としては、例えば、カーボンペースト、銀ペースト等の導電性ペーストを用いて陰極13を形成する方法、アルミニウム箔等の金属箔を誘電体層12に対向配置させる方法などが挙げられる。
The cathode forming step is a step of disposing the cathode 13 at a position facing the dielectric layer 12.
Examples of the method of arranging the cathode 13 include a method of forming the cathode 13 using a conductive paste such as carbon paste and silver paste, and a method of arranging a metal foil such as an aluminum foil opposite to the dielectric layer 12. It is done.

第一の固体電解質層形成工程は、誘電体層12の表面の少なくとも一部に、前記式(1)で表されるアジン化合物を含む溶液を塗布し、乾燥させて、第一の固体電解質層を形成する工程である。
前記溶液には、前記式(1)に該当しない前記含窒素化合物、後述する添加剤を含有させてもよい。
In the first solid electrolyte layer forming step, a solution containing the azine compound represented by the formula (1) is applied to at least a part of the surface of the dielectric layer 12 and dried to form a first solid electrolyte layer. Is a step of forming.
You may make the said solution contain the said nitrogen-containing compound which does not correspond to the said Formula (1), and the additive mentioned later.

前記アジン化合物を含む前記溶液を構成する溶媒は、前記アジン化合物を溶解又は分散させ得るもので、前記アジン化合物と反応しないものであれば特に限定されず、例えば、水、有機溶剤、又は、水と有機溶剤との混合液が挙げられる。前記有機溶剤の具体例としては、後述する導電性高分子分散液を構成する有機溶剤と同じものが挙げられる。それらの中でも、前記アジン化合物を安定に塗布できることから、水又は酢酸水溶液が好ましい。
前記酢酸水溶液の酢酸濃度は、例えば、0.01M以上1M以下が好ましく、0.05M以上0.5M以下がより好ましく、0.1M以上0.3M以下がさらに好ましい。
The solvent constituting the solution containing the azine compound is not particularly limited as long as it can dissolve or disperse the azine compound and does not react with the azine compound. For example, water, an organic solvent, or water And a mixed solution of an organic solvent. Specific examples of the organic solvent include the same organic solvents that constitute the conductive polymer dispersion described later. Among these, water or an aqueous acetic acid solution is preferable because the azine compound can be stably applied.
The acetic acid concentration of the acetic acid aqueous solution is, for example, preferably 0.01 M or more and 1 M or less, more preferably 0.05 M or more and 0.5 M or less, and further preferably 0.1 M or more and 0.3 M or less.

前記溶液の総質量に対する前記アジン化合物の含有量は特に限定されず、塗布することが容易な粘度となる含有量が好ましい。具体的には、例えば、0.1質量%以上10質量%以下が好ましく、0.3質量%以上5質量%以下がより好ましく、0.5質量%以上3質量%以下がさらに好ましい。
前記溶液が後述する添加剤を含有する場合、その含有量は、添加剤の種類に応じて適宜決められる。具体的には、例えば、前記溶液の総質量に対して、0.01質量%以上10質量%以下とすることができる。
Content of the said azine compound with respect to the total mass of the said solution is not specifically limited, Content which becomes the viscosity which is easy to apply | coat is preferable. Specifically, for example, 0.1% by mass to 10% by mass is preferable, 0.3% by mass to 5% by mass is more preferable, and 0.5% by mass to 3% by mass is more preferable.
When the said solution contains the additive mentioned later, the content is suitably determined according to the kind of additive. Specifically, for example, it can be 0.01% by mass or more and 10% by mass or less with respect to the total mass of the solution.

前記溶液は常法により調製され、例えば、溶媒に前記アジン化合物及び任意の添加剤を投入して、撹拌及び混合することにより調製される。   The solution is prepared by a conventional method, for example, by adding the azine compound and an arbitrary additive to a solvent, and stirring and mixing.

前記溶液の塗布方法としては、例えば、浸漬(ディップコーティング)、コンマコーティング、リバースコーティング、リップコーティング、マイクログラビアコーティング等を適用することができる。これらの中でも、誘電体層12と陰極13との間に第一の固体電解質層を容易に形成できる観点から、浸漬が好ましい。
乾燥方法としては、例えば、室温乾燥、熱風乾燥、遠赤外線乾燥等が挙げられる。
As a method for applying the solution, for example, dipping (dip coating), comma coating, reverse coating, lip coating, microgravure coating, or the like can be applied. Among these, dipping is preferable from the viewpoint that the first solid electrolyte layer can be easily formed between the dielectric layer 12 and the cathode 13.
Examples of the drying method include room temperature drying, hot air drying, and far infrared drying.

第二の固体電解質層形成工程は、第一の固体電解質層の表面の少なくとも一部に、π共役系導電性高分子及びポリアニオンを含む導電性複合体が分散された導電性高分子分散液を塗布し、乾燥させて、第二の固体電解質層を形成する工程である。
前段の工程において誘電体12の表面の一部のみが第一の固体電解質層によって覆われている場合には、第一の固体電解質層に覆われずに残った誘電体12の表面が第二の固体電解質層によって覆われてもよい。
前記導電性高分子分散液には、前記式(1)に該当しない前記含窒素化合物、後述する添加剤を含有させてもよい。一方、前記導電性高分子分散液に前記式(1)で表されるアジン化合物を添加すると、凝集が発生して塗布し難い状態になる場合があるので、前記アジン化合物を前記導電性高分子分散液に添加しない方がよい。
In the second solid electrolyte layer forming step, a conductive polymer dispersion in which a conductive complex containing a π-conjugated conductive polymer and a polyanion is dispersed on at least a part of the surface of the first solid electrolyte layer. It is a step of applying and drying to form a second solid electrolyte layer.
When only a part of the surface of the dielectric 12 is covered by the first solid electrolyte layer in the previous step, the surface of the dielectric 12 remaining without being covered by the first solid electrolyte layer is the second surface. The solid electrolyte layer may be covered.
The conductive polymer dispersion may contain the nitrogen-containing compound that does not correspond to the formula (1) and an additive that will be described later. On the other hand, when the azine compound represented by the formula (1) is added to the conductive polymer dispersion, aggregation may occur and it may be difficult to apply the azine compound. It is better not to add it to the dispersion.

導電性高分子分散液を構成する分散媒は、前記導電性複合体を分散させ得る液体であれば特に限定されず、例えば、水、有機溶剤、又は、水と有機溶剤との混合液が挙げられる。
有機溶剤としては、例えば、アルコール系溶媒、エーテル系溶媒、ケトン系溶媒、エステル系溶媒、芳香族炭化水素系溶媒等が挙げられる。これら有機溶剤は1種を単独で使用してもよいし、2種以上を併用してもよい。
アルコール系溶媒としては、例えば、メタノール、エタノール、イソプロパノール、n−ブタノール、t−ブタノール、アリルアルコール等が挙げられる。
エーテル系溶媒としては、例えば、ジエチルエーテル、ジメチルエーテル、エチレングリコール、プロピレングリコール、プロプレングリコールモノメチルエーテル等のプロピレングリコールモノアルキルエーテル、プロピレングリコールジアルキルエーテル等が挙げられる。
ケトン系溶媒としては、例えば、ジエチルケトン、メチルプロピルケトン、メチルブチルケトン、メチルイソプロピルケトン、メチルイソブチルケトン、メチルアミルケトン、ジイソプロピルケトン、メチルエチルケトン、アセトン、ジアセトンアルコール等が挙げられる。
エステル系溶媒としては、例えば、酢酸エチル、酢酸プロピル、酢酸ブチル等が挙げられる。
芳香族炭化水素系溶媒としては、例えば、ベンゼン、トルエン、キシレン、エチルベンゼン、プロピルベンゼン、イソプロピルベンゼン等が挙げられる。
The dispersion medium constituting the conductive polymer dispersion is not particularly limited as long as it is a liquid that can disperse the conductive composite, and examples thereof include water, an organic solvent, or a mixture of water and an organic solvent. It is done.
Examples of the organic solvent include alcohol solvents, ether solvents, ketone solvents, ester solvents, aromatic hydrocarbon solvents, and the like. These organic solvents may be used individually by 1 type, and may use 2 or more types together.
Examples of the alcohol solvent include methanol, ethanol, isopropanol, n-butanol, t-butanol, and allyl alcohol.
Examples of ether solvents include propylene glycol monoalkyl ethers such as diethyl ether, dimethyl ether, ethylene glycol, propylene glycol, and propylene glycol monomethyl ether, propylene glycol dialkyl ethers, and the like.
Examples of the ketone solvent include diethyl ketone, methyl propyl ketone, methyl butyl ketone, methyl isopropyl ketone, methyl isobutyl ketone, methyl amyl ketone, diisopropyl ketone, methyl ethyl ketone, acetone, diacetone alcohol and the like.
Examples of the ester solvent include ethyl acetate, propyl acetate, butyl acetate and the like.
Examples of the aromatic hydrocarbon solvent include benzene, toluene, xylene, ethylbenzene, propylbenzene, isopropylbenzene, and the like.

添加剤としては、例えば、界面活性剤、無機導電剤、消泡剤、カップリング剤、酸化防止剤、紫外線吸収剤などが挙げられる。ただし、添加剤は、前記導電性複合体、前記式(1)で表されるアジン化合物及び前記アジン化合物に該当しない前記含窒素化合物以外の化合物である。
界面活性剤としては、ノニオン系、アニオン系、カチオン系の界面活性剤が挙げられるが、保存安定性の面からノニオン系が好ましい。また、ポリビニルアルコール、ポリビニルピロリドンなどのポリマー系界面活性剤を添加してもよい。
無機導電剤としては、金属イオン類、導電性カーボン等が挙げられる。金属イオンは、金属塩を水に溶解させることにより生成させることができる。
消泡剤としては、シリコーン樹脂、ポリジメチルシロキサン、シリコーンオイル等が挙げられる。
カップリング剤としては、ビニル基、アミノ基、エポキシ基等を有するシランカップリング剤等が挙げられる。
酸化防止剤としては、フェノール系酸化防止剤、アミン系酸化防止剤、リン系酸化防止剤、硫黄系酸化防止剤、糖類等が挙げられる。
紫外線吸収剤としては、ベンゾトリアゾール系紫外線吸収剤、ベンゾフェノン系紫外線吸収剤、サリシレート系紫外線吸収剤、シアノアクリレート系紫外線吸収剤、オキサニリド系紫外線吸収剤、ヒンダードアミン系紫外線吸収剤、ベンゾエート系紫外線吸収剤等が挙げられる。
Examples of the additive include a surfactant, an inorganic conductive agent, an antifoaming agent, a coupling agent, an antioxidant, and an ultraviolet absorber. However, the additive is a compound other than the conductive complex, the azine compound represented by the formula (1), and the nitrogen-containing compound not corresponding to the azine compound.
Examples of the surfactant include nonionic, anionic and cationic surfactants, and nonionic surfactants are preferred from the viewpoint of storage stability. Moreover, you may add polymer type surfactants, such as polyvinyl alcohol and polyvinylpyrrolidone.
Examples of the inorganic conductive agent include metal ions and conductive carbon. Metal ions can be generated by dissolving a metal salt in water.
Examples of the antifoaming agent include silicone resin, polydimethylsiloxane, and silicone oil.
Examples of the coupling agent include silane coupling agents having a vinyl group, an amino group, an epoxy group, and the like.
Examples of the antioxidant include phenolic antioxidants, amine antioxidants, phosphorus antioxidants, sulfur antioxidants, and saccharides.
Examples of UV absorbers include benzotriazole UV absorbers, benzophenone UV absorbers, salicylate UV absorbers, cyanoacrylate UV absorbers, oxanilide UV absorbers, hindered amine UV absorbers, and benzoate UV absorbers. Is mentioned.

導電性高分子分散液の総質量に対する前記導電性複合体の含有量は特に限定されず、塗布することが容易な粘度となる含有量が好ましい。具体的には、例えば、0.01質量%以上10質量%以下が好ましく、0.1質量%以上5質量%以下がより好ましく、0.1質量%以上3質量%以下がさらに好ましい。
導電性高分子分散液が前記添加剤を含有する場合、その含有割合は、添加剤の種類に応じて適宜決められるが、例えば、導電性複合体の固形分100質量部に対して、0.1質量部以上500質量部以下の範囲内とすることができる。
The content of the conductive composite with respect to the total mass of the conductive polymer dispersion is not particularly limited, and is preferably a content that provides a viscosity that can be easily applied. Specifically, for example, 0.01% by mass to 10% by mass is preferable, 0.1% by mass to 5% by mass is more preferable, and 0.1% by mass to 3% by mass is more preferable.
When the conductive polymer dispersion contains the additive, the content is appropriately determined according to the type of the additive. For example, the content is 0. 10 parts by mass with respect to 100 parts by mass of the solid content of the conductive composite. It can be in the range of 1 to 500 parts by mass.

導電性高分子分散液の調製方法としては、ポリアニオン及び分散媒の存在下、π共役系導電性高分子を形成する前駆体モノマーを酸化重合する方法が挙げられる。前記式(1)に該当しない含窒素化合物及び添加剤の一方又は両方を添加する場合、それらの添加タイミングに特に制限はない。   Examples of a method for preparing the conductive polymer dispersion include a method in which a precursor monomer that forms a π-conjugated conductive polymer is oxidatively polymerized in the presence of a polyanion and a dispersion medium. In the case of adding one or both of the nitrogen-containing compound and the additive not corresponding to the formula (1), there is no particular limitation on the addition timing.

導電性高分子分散液の塗布方法は、前述した溶液の塗布方法と同様の方法が挙げられる。それらの中でも、第一の固体電解質層と陰極13との間に第二の固体電解質層を容易に形成できる観点から、浸漬が好ましい。
乾燥方法としては、例えば、室温乾燥、熱風乾燥、遠赤外線乾燥等が挙げられる。
Examples of the method for applying the conductive polymer dispersion include the same method as the method for applying the solution described above. Among these, dipping is preferable from the viewpoint that the second solid electrolyte layer can be easily formed between the first solid electrolyte layer and the cathode 13.
Examples of the drying method include room temperature drying, hot air drying, and far infrared drying.

本発明のキャパシタ及びその製造方法は上記の実施形態の例に限定されない。
本発明のキャパシタでは、誘電体層と陰極との間に、セパレータが設けられてもよい。誘電体層と陰極との間にセパレータが設けられたキャパシタとしては、巻回型キャパシタが挙げられる。
セパレータとしては、例えば、ポリビニルアルコール、ポリエステル、ポリエチレン、ポリスチレン、ポリプロピレン、ポリイミド、ポリアミド、ポリフッ化ビニリデンなどからなるシート(不織布を含む)、ガラス繊維の不織布などが挙げられる。
セパレータの密度は、0.1g/cm以上1.0g/cm以下の範囲であることが好ましく、0.2g/cm以上0.8g/cm以下の範囲であることがより好ましい。
セパレータを設ける場合には、セパレータにカーボンペーストあるいは銀ペーストを含浸させて陰極を形成する方法を適用することもできる。
The capacitor and the manufacturing method thereof according to the present invention are not limited to the above-described embodiments.
In the capacitor of the present invention, a separator may be provided between the dielectric layer and the cathode. Examples of the capacitor in which a separator is provided between the dielectric layer and the cathode include a wound capacitor.
Examples of the separator include sheets (including non-woven fabric) made of polyvinyl alcohol, polyester, polyethylene, polystyrene, polypropylene, polyimide, polyamide, polyvinylidene fluoride, and non-woven fabric of glass fiber.
The density of the separator is more preferably it is 0.1 g / cm 3 or more 1.0 g / cm 3 or less in the range is preferable, 0.2 g / cm 3 or more 0.8 g / cm 3 or less.
In the case of providing a separator, a method of forming a cathode by impregnating the separator with a carbon paste or a silver paste can also be applied.

(製造例1)
1000mlのイオン交換水に206gのスチレンスルホン酸ナトリウムを溶解し、80℃で攪拌しながら、予め10mlの水に溶解した1.14gの過硫酸アンモニウム酸化剤溶液を20分間滴下し、この溶液を12時間攪拌した。
得られたスチレンスルホン酸ナトリウム含有溶液に10質量%に希釈した硫酸を1000ml添加し、限外ろ過法によりポリスチレンスルホン酸含有溶液の約1000ml溶液を除去し、残液に2000mlのイオン交換水を加え、限外ろ過法により約2000ml溶液を除去した。上記の限外ろ過操作を3回繰り返した。さらに、得られたろ液に約2000mlのイオン交換水を添加し、限外ろ過法により約2000mlの溶液を除去した。この限外ろ過操作を3回繰り返した。
得られた溶液中の水を減圧除去して、無色の固形状のポリスチレンスルホン酸を得た。
(Production Example 1)
Dissolve 206 g of sodium styrenesulfonate in 1000 ml of ion-exchanged water and, while stirring at 80 ° C., add dropwise 1.14 g of ammonium persulfate oxidizer solution previously dissolved in 10 ml of water for 20 minutes. Stir.
To the obtained sodium styrenesulfonate-containing solution, 1000 ml of sulfuric acid diluted to 10% by mass was added, about 1000 ml of the polystyrenesulfonic acid-containing solution was removed by ultrafiltration, and 2000 ml of ion-exchanged water was added to the remaining liquid. About 2000 ml of solution was removed by ultrafiltration. The above ultrafiltration operation was repeated three times. Further, about 2000 ml of ion-exchanged water was added to the obtained filtrate, and about 2000 ml of the solution was removed by ultrafiltration. This ultrafiltration operation was repeated three times.
Water in the obtained solution was removed under reduced pressure to obtain colorless solid polystyrene sulfonic acid.

(製造例2)
3,4−エチレンジオキシチオフェン14.2gと、製造例1で得たポリスチレンスルホン酸36.7gとを2000mlのイオン交換水に溶かした溶液とを20℃で混合させた。
これにより得られた混合溶液を20℃に保ち、掻き混ぜながら、200mlのイオン交換水に溶かした29.64gの過硫酸アンモニウムと8.0gの硫酸第二鉄の酸化触媒溶液とをゆっくり添加し、3時間攪拌して反応させた。
得られた反応液に2000mlのイオン交換水を加え、限外ろ過法により約2000ml溶液を除去した。この操作を3回繰り返した。
そして、得られた溶液に200mlの10質量%に希釈した硫酸と2000mlのイオン交換水とを加え、限外ろ過法により約2000mlの溶液を除去し、これに2000mlのイオン交換水を加え、限外ろ過法により約2000ml溶液を除去した。この操作を3回繰り返した。
さらに、得られた溶液に2000mlのイオン交換水を加え、限外ろ過法により約2000mlの溶液を除去した。この操作を5回繰り返したのち、高圧分散機を用い、140MPaの圧力で分散処理を施して、1.4質量%のポリスチレンスルホン酸ドープポリ(3,4−エチレンジオキシチオフェン)水分散液(PEDOT−PSS水分散液)を得た。
(Production Example 2)
A solution prepared by dissolving 14.2 g of 3,4-ethylenedioxythiophene and 36.7 g of the polystyrene sulfonic acid obtained in Production Example 1 in 2000 ml of ion-exchanged water was mixed at 20 ° C.
While maintaining the mixed solution thus obtained at 20 ° C. and stirring, 29.64 g of ammonium persulfate dissolved in 200 ml of ion exchange water and 8.0 g of ferric sulfate oxidation catalyst solution were slowly added, The reaction was stirred for 3 hours.
2000 ml of ion-exchanged water was added to the obtained reaction solution, and about 2000 ml of solution was removed by ultrafiltration. This operation was repeated three times.
Then, 200 ml of sulfuric acid diluted to 10% by mass and 2000 ml of ion-exchanged water are added to the resulting solution, about 2000 ml of solution is removed by ultrafiltration, and 2000 ml of ion-exchanged water is added to this solution. About 2000 ml of solution was removed by external filtration. This operation was repeated three times.
Furthermore, 2000 ml of ion-exchanged water was added to the obtained solution, and about 2000 ml of the solution was removed by ultrafiltration. After repeating this operation five times, the dispersion treatment was performed at a pressure of 140 MPa using a high-pressure disperser, and a 1.4% by weight polystyrenesulfonic acid-doped poly (3,4-ethylenedioxythiophene) aqueous dispersion (PEDOT). -PSS aqueous dispersion).

(製造例3)
エッチドアルミニウム箔(陽極箔)に陽極リード端子を接続した後、アジピン酸アンモニウム10質量%水溶液中で80Vの電圧を印加し、化成(酸化処理)して、アルミニウム箔の両面に誘電体層を形成して陽極箔を得た。
次に、陽極箔の両面に、陰極リード端子を溶接させた対向アルミニウム陰極箔を、セルロース製のセパレータを介して積層し、これを円筒状に巻き取ってキャパシタ用素子を得た。
(Production Example 3)
After connecting the anode lead terminal to the etched aluminum foil (anode foil), a voltage of 80 V was applied in an aqueous solution of 10% by weight ammonium adipate to form (oxidize) the dielectric layer on both sides of the aluminum foil. An anode foil was obtained by forming.
Next, on both surfaces of the anode foil, an opposing aluminum cathode foil with cathode lead terminals welded was laminated via a cellulose separator, and this was wound into a cylindrical shape to obtain a capacitor element.

(実施例1)
イオン交換水99.7質量部にメラミン0.3質量部を溶かしてアジン化合物の水溶液を得た。この水溶液を、製造例3で得たキャパシタ用素子に減圧下で浸漬した後、125℃の熱風乾燥機により15分間乾燥し、誘電体層表面上にアジン化合物を含む固体電解質層(第一の固体電解質層)を形成させた。
次いで、アジン化合物を含む固体電解質層を形成させたキャパシタ用素子を製造例2で得たPEDOT−PSS水分散液に減圧下で浸漬した後、125℃の熱風乾燥機により15分間乾燥し、誘電体層表面上及び第一の固体電解質層上に導電性複合体を含む第二の固体電解質層を形成させた。
さらに、アルミニウム製のケースに、第一及び第二の固体電解質層を形成したキャパシタ用素子を装填し、封口ゴムで封止して、キャパシタを得た。
Example 1
Melting 0.3 parts by mass of melamine in 99.7 parts by mass of ion-exchanged water gave an aqueous solution of an azine compound. This aqueous solution was immersed in the capacitor element obtained in Production Example 3 under reduced pressure, and then dried for 15 minutes with a hot air dryer at 125 ° C., and the solid electrolyte layer containing the azine compound on the surface of the dielectric layer (first A solid electrolyte layer) was formed.
Next, the capacitor element on which the solid electrolyte layer containing the azine compound was formed was immersed in the PEDOT-PSS aqueous dispersion obtained in Production Example 2 under reduced pressure, and then dried by a hot air dryer at 125 ° C. for 15 minutes. A second solid electrolyte layer containing a conductive composite was formed on the surface of the body layer and on the first solid electrolyte layer.
Furthermore, the capacitor element in which the first and second solid electrolyte layers were formed was loaded in an aluminum case and sealed with a sealing rubber to obtain a capacitor.

(実施例2)
イオン交換水を0.1M酢酸水溶液に変更した他は、実施例1と同様にして、キャパシタを得た。
(Example 2)
A capacitor was obtained in the same manner as in Example 1 except that the ion-exchanged water was changed to a 0.1 M acetic acid aqueous solution.

(実施例3)
イオン交換水99.7質量部を0.1M酢酸水溶液99.0質量部に、メラミン0.3質量部を1.0質量部に変更した他は、実施例1と同様にして、キャパシタを得た。
(Example 3)
A capacitor was obtained in the same manner as in Example 1 except that 99.7 parts by mass of ion-exchanged water was changed to 99.0 parts by mass of 0.1M acetic acid aqueous solution and 0.3 part by mass of melamine was changed to 1.0 part by mass. It was.

(実施例4)
イオン交換水99.7質量部を0.1M酢酸水溶液98.7質量部に、メラミン0.3質量部を1.3質量部に変更した他は、実施例1と同様にして、キャパシタを得た。
Example 4
A capacitor was obtained in the same manner as in Example 1 except that 99.7 parts by mass of ion-exchanged water was changed to 98.7 parts by mass of 0.1M acetic acid aqueous solution and 0.3 part by mass of melamine was changed to 1.3 parts by mass. It was.

(実施例5)
イオン交換水99.7質量部を99.9質量部に、メラミン0.3質量部を0.1質量部に変更した他は、実施例1と同様にして、キャパシタを得た。
(Example 5)
A capacitor was obtained in the same manner as in Example 1 except that 99.7 parts by mass of ion-exchanged water was changed to 99.9 parts by mass and 0.3 parts by mass of melamine was changed to 0.1 parts by mass.

(実施例6)
イオン交換水を0.1M酢酸水溶液に、メラミンをアセトグアナミンに変更した他は、実施例1と同様にして、キャパシタを得た。
(Example 6)
A capacitor was obtained in the same manner as in Example 1 except that the ion exchange water was changed to 0.1 M acetic acid aqueous solution and the melamine was changed to acetoguanamine.

(実施例7)
イオン交換水99.7質量部を0.1M酢酸水溶液99.9質量部に、メラミン0.3質量部をアセトグアナミン0.1質量部に変更した他は、実施例1と同様にして、キャパシタを得た。
(Example 7)
A capacitor was obtained in the same manner as in Example 1 except that 99.7 parts by mass of ion-exchanged water was changed to 99.9 parts by mass of 0.1M acetic acid aqueous solution, and 0.3 part by mass of melamine was changed to 0.1 parts by mass of acetoguanamine Got.

(実施例8)
メラミン0.3質量部を2,4,6−[トリス(ビスメトキシメチル)アミノ]1,3,5−トリアジン0.3質量部に変更した他は、実施例1と同様にして、キャパシタを得た。
(Example 8)
In the same manner as in Example 1, except that 0.3 part by mass of melamine was changed to 0.3 part by mass of 2,4,6- [tris (bismethoxymethyl) amino] 1,3,5-triazine. Obtained.

(実施例9)
イオン交換水99.7質量部を99.0質量部に、メラミン0.3質量部を2,4,6−[トリス(ビスメトキシメチル)アミノ]1,3,5−トリアジン1.0質量部に変更した他は、実施例1と同様にして、キャパシタを得た。
Example 9
99.7 parts by mass of ion-exchanged water is 99.0 parts by mass, 0.3 parts by mass of melamine is 1.0 part by mass of 2,4,6- [tris (bismethoxymethyl) amino] 1,3,5-triazine. A capacitor was obtained in the same manner as in Example 1 except that the capacitor was changed.

(実施例10)
メラミン0.3質量部を2,4,6−トリアミノピリミジン0.3質量部に変更した他は、実施例1と同様にして、キャパシタを得た。
(Example 10)
A capacitor was obtained in the same manner as in Example 1 except that 0.3 part by mass of melamine was changed to 0.3 part by mass of 2,4,6-triaminopyrimidine.

(実施例11)
メラミン0.3質量部を2−アミノピリミジン0.3質量部に変更した他は、実施例1と同様にして、キャパシタを得た。
(Example 11)
A capacitor was obtained in the same manner as in Example 1 except that 0.3 part by mass of melamine was changed to 0.3 part by mass of 2-aminopyrimidine.

(実施例12)
メラミン0.3質量部をp−アミノピリジン(4−アミノピリジン)0.3質量部に変更した他は、実施例1と同様にして、キャパシタを得た。
(Example 12)
A capacitor was obtained in the same manner as in Example 1 except that 0.3 part by mass of melamine was changed to 0.3 part by mass of p-aminopyridine (4-aminopyridine).

(実施例13)
メラミン0.3質量部をN,N−ジメチル−4−アミノピリジン(DMAP)0.3質量部に変更した他は、実施例1と同様にして、キャパシタを得た。
(Example 13)
A capacitor was obtained in the same manner as in Example 1 except that 0.3 part by mass of melamine was changed to 0.3 part by mass of N, N-dimethyl-4-aminopyridine (DMAP).

(実施例14)
アジン化合物の水溶液を、イオン交換水99.6質量部にメラミン0.3質量部及びイミダゾール0.1質量部を溶かして得たアジン化合物の水溶液に変更した他は、実施例1と同様にして、キャパシタを得た。
(Example 14)
Except having changed the aqueous solution of an azine compound into the aqueous solution of the azine compound obtained by melt | dissolving 0.3 mass part of melamine and 0.1 mass part of imidazole in 99.6 mass parts of ion-exchange water, it carried out similarly to Example 1. A capacitor was obtained.

(実施例15)
アジン化合物の水溶液を、イオン交換水99.6質量部にメラミン0.3質量部及びトリエチルアミン0.1質量部を溶かして得たアジン化合物の水溶液に変更した他は、実施例1と同様にして、キャパシタを得た。
(Example 15)
The aqueous solution of the azine compound was changed to an aqueous solution of the azine compound obtained by dissolving 0.3 part by mass of melamine and 0.1 part by mass of triethylamine in 99.6 parts by mass of ion-exchanged water, in the same manner as in Example 1. A capacitor was obtained.

(実施例16)
アジン化合物の水溶液を、イオン交換水99.6質量部にメラミン0.3質量部及びトリプロピルアミン0.1質量部を溶かして得たアジン化合物の水溶液に変更した他は、実施例1と同様にして、キャパシタを得た。
(Example 16)
The same as in Example 1 except that the aqueous solution of the azine compound was changed to an aqueous solution of the azine compound obtained by dissolving 0.3 part by mass of melamine and 0.1 part by mass of tripropylamine in 99.6 parts by mass of ion-exchanged water. Thus, a capacitor was obtained.

(比較例1)
メラミン0.3質量部をイミダゾール0.3質量部に変更した他は、実施例1と同様にして、キャパシタを得た。
(Comparative Example 1)
A capacitor was obtained in the same manner as in Example 1 except that 0.3 part by mass of melamine was changed to 0.3 part by mass of imidazole.

(比較例2)
イオン交換水99.7質量部を99.9質量部に、トリエチルアミン0.1質量部に変更した他は、実施例1と同様にして、キャパシタを得た。
(Comparative Example 2)
A capacitor was obtained in the same manner as in Example 1 except that 99.7 parts by mass of ion-exchanged water was changed to 99.9 parts by mass and 0.1 parts by mass of triethylamine.

(比較例3)
メラミンを含まなかった以外は、実施例1と同様にして、キャパシタを得た。
(Comparative Example 3)
A capacitor was obtained in the same manner as in Example 1 except that melamine was not included.

(比較例4)
メラミンを含まなかった以外は、実施例2と同様にして、キャパシタを得た。
(Comparative Example 4)
A capacitor was obtained in the same manner as in Example 2 except that melamine was not included.

(実施例17)
イオン交換水99.7質量部にメラミン0.3質量部を溶かしてアジン化合物の水溶液を得た。この水溶液を、製造例3で得たキャパシタ用素子に減圧下で浸漬した後、125℃の熱風乾燥機により15分間乾燥し、誘電体層表面上にアジン化合物を含む固体電解質層(第一の固体電解質層)を形成させた。
次いで、製造例2で得たPEDOT−PSS水分散液100質量部にイミダゾール0.05質量部を加えて含窒素化合物を含むPEDOT−PSS水分散液を調製した。
アジン化合物を含む固体電解質層を形成させたキャパシタ用素子に、含窒素化合物を含むPEDOT−PSS水分散液を減圧下で浸漬した後、125℃の熱風乾燥機により15分間乾燥し、誘電体層表面上及び第一の固体電解質層上に導電性複合体を含む第二の固体電解質層を形成させた。
さらに、アルミニウム製のケースに、第一及び第二の固体電解質層を形成したキャパシタ用素子を装填し、封口ゴムで封止して、キャパシタを得た。
(Example 17)
Melting 0.3 parts by mass of melamine in 99.7 parts by mass of ion-exchanged water gave an aqueous solution of an azine compound. This aqueous solution was immersed in the capacitor element obtained in Production Example 3 under reduced pressure, and then dried for 15 minutes with a hot air dryer at 125 ° C., and the solid electrolyte layer containing the azine compound on the surface of the dielectric layer (first A solid electrolyte layer) was formed.
Next, 0.05 part by mass of imidazole was added to 100 parts by mass of the PEDOT-PSS aqueous dispersion obtained in Production Example 2 to prepare a PEDOT-PSS aqueous dispersion containing a nitrogen-containing compound.
After immersing a PEDOT-PSS aqueous dispersion containing a nitrogen-containing compound in a capacitor element having a solid electrolyte layer containing an azine compound under reduced pressure, the dielectric layer is dried for 15 minutes by a hot air dryer at 125 ° C. A second solid electrolyte layer containing a conductive composite was formed on the surface and on the first solid electrolyte layer.
Furthermore, the capacitor element in which the first and second solid electrolyte layers were formed was loaded in an aluminum case and sealed with a sealing rubber to obtain a capacitor.

(実施例18)
イミダゾール0.05質量部を0.1質量部に変更した他は、実施例17と同様にして、キャパシタを得た。
(Example 18)
A capacitor was obtained in the same manner as in Example 17 except that 0.05 part by mass of imidazole was changed to 0.1 part by mass.

(実施例19)
イミダゾール0.05質量部を0.25質量部に変更した他は、実施例17と同様にして、キャパシタを得た。
(Example 19)
A capacitor was obtained in the same manner as in Example 17 except that 0.05 part by mass of imidazole was changed to 0.25 part by mass.

(実施例20)
イミダゾール0.05質量部をトリエチルアミン0.05質量部に変更した他は、実施例17と同様にして、キャパシタを得た。
(Example 20)
A capacitor was obtained in the same manner as in Example 17 except that 0.05 part by mass of imidazole was changed to 0.05 part by mass of triethylamine.

(実施例21)
イミダゾール0.05質量部をトリエチルアミン0.1質量部に変更した他は、実施例17と同様にして、キャパシタを得た。
(Example 21)
A capacitor was obtained in the same manner as in Example 17 except that 0.05 part by mass of imidazole was changed to 0.1 part by mass of triethylamine.

(実施例22)
イミダゾール0.05質量部をトリプロピルアミン0.05質量部に変更した他は、実施例17と同様にして、キャパシタを得た。
(Example 22)
A capacitor was obtained in the same manner as in Example 17 except that 0.05 part by mass of imidazole was changed to 0.05 part by mass of tripropylamine.

(実施例23)
イミダゾール0.05質量部をトリプロピルアミン0.1質量部に変更した他は、実施例17と同様にして、キャパシタを得た。
(Example 23)
A capacitor was obtained in the same manner as in Example 17 except that 0.05 part by mass of imidazole was changed to 0.1 part by mass of tripropylamine.

<評価>
得られた各例のキャパシタについて、LCRメータZM2376((株)エヌエフ回路設計ブロック製)を用いて、120Hzでの静電容量、及び100kHzでの等価直列抵抗を測定した。120Hzでの静電容量、及び100kHzでの等価直列抵抗(ESR)の測定結果を表1に示す。
<Evaluation>
About the obtained capacitor of each example, the electrostatic capacity in 120 Hz and the equivalent series resistance in 100 kHz were measured using LCR meter ZM2376 (made by NF circuit design block). Table 1 shows the measurement results of capacitance at 120 Hz and equivalent series resistance (ESR) at 100 kHz.

Figure 2018085420
Figure 2018085420

前記式(1)で表されるアジン化合物を含む第一の固体電解質層をキャパシタ素子の誘電体表面に形成した実施例1〜13では、得られたキャパシタが充分な静電容量を有しつつ、等価直列抵抗が充分に小さかった。
上記アジン化合物を含有しない第一の固体電解質層をキャパシタ素子の誘電体表面に形成した比較例1〜4では、得られたキャパシタの等価直列抵抗が大きかった。
In Examples 1 to 13 in which the first solid electrolyte layer containing the azine compound represented by the formula (1) was formed on the dielectric surface of the capacitor element, the obtained capacitors had sufficient capacitance. The equivalent series resistance was sufficiently small.
In Comparative Examples 1 to 4 in which the first solid electrolyte layer not containing the azine compound was formed on the dielectric surface of the capacitor element, the equivalent series resistance of the obtained capacitor was large.

実施例14〜16では、前記式(1)で表されるアジン化合物だけでなく、前記式(1)に該当しない含窒素化合物も合わせて含む第一の固体電解質層をキャパシタ素子の誘電体表面に形成した。その結果、得られたキャパシタの静電容量が増加し、等価直列抵抗がより小さくなる傾向が確認された。
実施例17〜23では、導電性複合体のPEDOT−PSSだけでなく、前記式(1)に該当しない含窒素化合物を添加した第二の固体電解質層を、誘電体層を覆う第一の固体電解質層の上に形成した。その結果、得られたキャパシタの静電容量が増加し、等価直列抵抗がより小さくなる傾向が確認された。
In Examples 14 to 16, the first solid electrolyte layer containing not only the azine compound represented by the formula (1) but also a nitrogen-containing compound not corresponding to the formula (1) is included in the dielectric surface of the capacitor element. Formed. As a result, it was confirmed that the capacitance of the obtained capacitor increased and the equivalent series resistance tended to be smaller.
In Examples 17 to 23, the second solid electrolyte layer to which the nitrogen-containing compound not corresponding to the formula (1) was added as well as the PEDOT-PSS of the conductive composite was used as the first solid covering the dielectric layer. It formed on the electrolyte layer. As a result, it was confirmed that the capacitance of the obtained capacitor increased and the equivalent series resistance tended to be smaller.

10 キャパシタ
11 陽極
12 誘電体層
13 陰極
14 固体電解質層
10 Capacitor 11 Anode 12 Dielectric Layer 13 Cathode 14 Solid Electrolyte Layer

Claims (14)

弁金属の多孔質体からなる陽極と、前記弁金属の酸化物からなる誘電体層と、前記誘電体層の、前記陽極と反対側に設けられた導電物質製の陰極と、前記誘電体層及び前記陰極の間に設けられた少なくとも1層の固体電解質層とを具備し、
前記固体電解質層が、π共役系導電性高分子及びポリアニオンを含む導電性複合体と、下記式(1)で表されるアジン化合物とを含有する、キャパシタ。
Figure 2018085420
[式(1)中、X,X,Xは各々独立してCH又はNであり、R,R,Rは各々独立して水素原子又は任意の置換基であり、X,X,Xのうち少なくとも何れか1つはNであり、R,R,Rのうち少なくとも何れか1つは窒素を有する置換基である。]
An anode made of a porous body of a valve metal, a dielectric layer made of an oxide of the valve metal, a cathode made of a conductive material provided on the opposite side of the dielectric layer from the anode, and the dielectric layer And at least one solid electrolyte layer provided between the cathodes,
The capacitor in which the solid electrolyte layer contains a conductive composite containing a π-conjugated conductive polymer and a polyanion, and an azine compound represented by the following formula (1).
Figure 2018085420
[In the formula (1), X 1 , X 2 and X 3 are each independently CH or N, R 1 , R 2 and R 3 are each independently a hydrogen atom or an arbitrary substituent; At least one of 1 , X 2 and X 3 is N, and at least one of R 1 , R 2 and R 3 is a nitrogen-containing substituent. ]
前記固体電解質層は、前記誘電体層の少なくとも一部を覆う第一の固体電解質層と、前記第一の固体電解質層の少なくとも一部を覆う第二の固体電解質層と、を有する、請求項1に記載のキャパシタ。   The solid electrolyte layer has a first solid electrolyte layer covering at least a part of the dielectric layer, and a second solid electrolyte layer covering at least a part of the first solid electrolyte layer. The capacitor according to 1. 前記第一の固体電解質層は前記アジン化合物を含み、前記第二の固体電解質層は前記導電性複合体を含む、請求項2に記載のキャパシタ。   The capacitor according to claim 2, wherein the first solid electrolyte layer includes the azine compound, and the second solid electrolyte layer includes the conductive composite. 前記固体電解質層が、前記式(1)に該当しない含窒素化合物をさらに含有する、請求項1〜3の何れか一項に記載のキャパシタ。   The capacitor according to any one of claims 1 to 3, wherein the solid electrolyte layer further contains a nitrogen-containing compound not corresponding to the formula (1). 前記式(1)に該当しない前記含窒素化合物が、イミダゾール、トリエチルアミン、及びトリプロピルアミンから選ばれる何れか1つ以上である、請求項4に記載のキャパシタ。   The capacitor according to claim 4, wherein the nitrogen-containing compound not corresponding to the formula (1) is any one or more selected from imidazole, triethylamine, and tripropylamine. 前記式(1)中、R,R,Rのうち少なくとも何れか1つはアミノ基である、請求項1〜5の何れか一項に記載のキャパシタ。 The capacitor according to claim 1 , wherein in the formula (1), at least one of R 1 , R 2 , and R 3 is an amino group. 前記π共役系導電性高分子が、ポリ(3,4−エチレンジオキシチオフェン)である、請求項1〜6の何れか一項に記載のキャパシタ。   The capacitor according to any one of claims 1 to 6, wherein the π-conjugated conductive polymer is poly (3,4-ethylenedioxythiophene). 前記ポリアニオンが、ポリスチレンスルホン酸である、請求項1〜7の何れか一項に記載のキャパシタ。   The capacitor according to claim 1, wherein the polyanion is polystyrene sulfonic acid. 弁金属の多孔質体からなる陽極の表面を酸化して誘電体層を形成する工程と、
前記誘電体層に対向する位置に陰極を配置する工程と、
前記誘電体層の表面の少なくとも一部に、下記式(1)で表されるアジン化合物を含む溶液を塗布し、乾燥させて、第一の固体電解質層を形成する工程と、
前記第一の固体電解質層の表面の少なくとも一部に、π共役系導電性高分子及びポリアニオンを含む導電性複合体が分散された導電性高分子分散液を塗布し、乾燥させて、第二の固体電解質層を形成する工程と、を有するキャパシタの製造方法。
Figure 2018085420
[式(1)中、X,X,Xは各々独立してCH又はNであり、R,R,Rは各々独立して水素原子又は任意の置換基であり、X,X,Xのうち少なくとも何れか1つはNであり、R,R,Rのうち少なくとも何れか1つは窒素を有する置換基である。]
Oxidizing the surface of the anode made of a porous body of valve metal to form a dielectric layer;
Disposing a cathode at a position facing the dielectric layer;
Applying a solution containing an azine compound represented by the following formula (1) to at least a part of the surface of the dielectric layer and drying to form a first solid electrolyte layer;
A conductive polymer dispersion liquid in which a conductive complex containing a π-conjugated conductive polymer and a polyanion is dispersed is applied to at least a part of the surface of the first solid electrolyte layer, and dried. Forming a solid electrolyte layer of the capacitor.
Figure 2018085420
[In the formula (1), X 1 , X 2 and X 3 are each independently CH or N, R 1 , R 2 and R 3 are each independently a hydrogen atom or an arbitrary substituent; At least one of 1 , X 2 and X 3 is N, and at least one of R 1 , R 2 and R 3 is a nitrogen-containing substituent. ]
前記溶液及び前記導電性高分子分散液のうち少なくとも一方が、前記式(1)に該当しない含窒素化合物を含む、請求項9に記載のキャパシタの製造方法。   The method for manufacturing a capacitor according to claim 9, wherein at least one of the solution and the conductive polymer dispersion contains a nitrogen-containing compound not corresponding to the formula (1). 前記式(1)に該当しない前記含窒素化合物が、イミダゾール、トリエチルアミン、及びトリプロピルアミンから選ばれる何れか1つ以上である、請求項10に記載のキャパシタの製造方法。   The method for manufacturing a capacitor according to claim 10, wherein the nitrogen-containing compound not corresponding to the formula (1) is one or more selected from imidazole, triethylamine, and tripropylamine. 前記式(1)中、R,R,Rのうち少なくとも何れか1つはアミノ基である、請求項9〜11の何れか一項に記載のキャパシタの製造方法。 12. The method for manufacturing a capacitor according to claim 9, wherein, in the formula (1), at least one of R 1 , R 2 , and R 3 is an amino group. 前記π共役系導電性高分子が、ポリ(3,4−エチレンジオキシチオフェン)である、請求項9〜12の何れか一項に記載のキャパシタの製造方法。   The method for producing a capacitor according to any one of claims 9 to 12, wherein the π-conjugated conductive polymer is poly (3,4-ethylenedioxythiophene). 前記ポリアニオンが、ポリスチレンスルホン酸である、請求項9〜13の何れか一項に記載のキャパシタの製造方法。   The method for producing a capacitor according to claim 9, wherein the polyanion is polystyrene sulfonic acid.
JP2016227185A 2016-11-22 2016-11-22 Capacitors and their manufacturing methods Active JP6820727B2 (en)