JP2016182808A - Decorative sheet - Google Patents

Decorative sheet Download PDF

Info

Publication number
JP2016182808A
JP2016182808A JP2015181148A JP2015181148A JP2016182808A JP 2016182808 A JP2016182808 A JP 2016182808A JP 2015181148 A JP2015181148 A JP 2015181148A JP 2015181148 A JP2015181148 A JP 2015181148A JP 2016182808 A JP2016182808 A JP 2016182808A
Authority
JP
Japan
Prior art keywords
layer
release layer
thermosetting resin
resin
decorative board
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
JP2015181148A
Other languages
Japanese (ja)
Other versions
JP6716877B2 (en
Inventor
明彦 片島
Akihiko Katajima
明彦 片島
小林 武
Takeshi Kobayashi
武 小林
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Dai Nippon Printing Co Ltd
Original Assignee
Dai Nippon Printing Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Dai Nippon Printing Co Ltd filed Critical Dai Nippon Printing Co Ltd
Priority to PCT/JP2016/057871 priority Critical patent/WO2016148091A1/en
Publication of JP2016182808A publication Critical patent/JP2016182808A/en
Application granted granted Critical
Publication of JP6716877B2 publication Critical patent/JP6716877B2/en
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

PROBLEM TO BE SOLVED: To provide a decorative sheet capable of expressing a design feeling of a clear gross mat tone, and easy in manufacture.SOLUTION: A decorative sheet has a release layer 2 in a partial area of a surface of a porous base material 1 such as a fibrous base material having thermosetting resin permeability and has a thermosetting resin layer 3 in a residual part area of a surface of the porous base material 1 having no release layer 2, and is laminated on a wooden base material such as an internal facing of a building such as a wall, the ceiling and a floor, furniture or a cabinet of a light current or OA equipment.SELECTED DRAWING: Figure 1

Description

本発明は、化粧板に関する。   The present invention relates to a decorative board.

従来、テーブル、カウンター、壁、床等の表面には、チタン紙等の多孔質基材にメラミン樹脂を含浸させ、必要に応じてフェノールコア紙等に積層した化粧板が積層されている。このようなメラミン樹脂を含浸させた化粧板は、強度、硬さ、耐熱性等の物性を示す。   Conventionally, a decorative board in which a porous base material such as titanium paper is impregnated with melamine resin and laminated on phenol core paper or the like is laminated on the surface of a table, counter, wall, floor or the like. A decorative board impregnated with such a melamine resin exhibits physical properties such as strength, hardness and heat resistance.

上述のような化粧板には、高級感を示す意匠が求められており、グロスマット調の意匠感を表面に付与することが行われている。   The decorative board as described above is required to have a high-quality design, and a glossy matte design is imparted to the surface.

表面にグロスマット調の意匠感が付与された化粧板として、表面にグロスマット調のエンボス形状が形成されたエンボス板(テクスチャーを付けた鏡面板)を用いて熱圧プレスされた化粧板が提案されている(例えば、特許文献1参照)。   A decorative board that has been hot-pressed using an embossed board with a glossy matte embossed shape on the surface (a mirrored board with a texture) is proposed as a decorative board with a glossy matte design. (For example, refer to Patent Document 1).

しかしながら、特許文献1に記載されている化粧板の表面にグロスマット調の意匠感を付与する場合、意匠の種類だけ表面処理した鏡面板が必要であり、コストがかかり製造が困難であるという問題がある。また、この化粧板は、エンボス形状を下地の絵柄と同調させることが困難であり、より意匠性を高めることが困難であるという問題がある。   However, when a glossy matte design feeling is imparted to the surface of the decorative plate described in Patent Document 1, a mirror plate that has been surface-treated only for the type of design is required, which is expensive and difficult to manufacture. There is. In addition, this decorative board has a problem that it is difficult to synchronize the embossed shape with the underlying pattern, and it is difficult to further improve the design.

また、絵柄模様と同調した凹状部等が形成された化粧板の製造方法として、原紙の表面に浸透防止層と撥液性模様層を設けることで熱硬化性樹脂を含浸して熱圧成形する際に、撥液性模様が熱硬化性樹脂の皮膜に被覆される現象を防止する製造方法が提案されている(例えば、特許文献2参照)。   In addition, as a method of manufacturing a decorative board in which concave portions or the like synchronized with a pattern are formed, a thermosetting resin is impregnated with a thermosetting resin by providing a permeation prevention layer and a liquid repellent pattern layer on the surface of the base paper. At the same time, a manufacturing method for preventing a phenomenon in which a liquid-repellent pattern is covered with a film of a thermosetting resin has been proposed (for example, see Patent Document 2).

しかしながら、特許文献2に記載されている製造方法では、完全に熱硬化性樹脂の被覆を防止することは困難であり、このような製造方法により製造された化粧板は、鮮明なグロスマット調の意匠感を表現することが困難であるという問題がある。   However, in the manufacturing method described in Patent Document 2, it is difficult to completely prevent the thermosetting resin from being coated, and the decorative board manufactured by such a manufacturing method has a clear gloss matte tone. There is a problem that it is difficult to express a sense of design.

従って、鮮明なグロスマット調の意匠感を表現することができ、製造が容易な化粧板の開発が望まれている。   Therefore, it is desired to develop a decorative board that can express a clear gloss matte design and is easy to manufacture.

特開昭47−14273号公報JP-A-47-14273 特開2002−166501号公報JP 2002-166501 A

本発明は、鮮明なグロスマット調の意匠感を表現することができ、製造が容易な化粧板を提供することを目的とする。   It is an object of the present invention to provide a decorative board that can express a clear gloss matte design and is easy to manufacture.

本発明者等は、鋭意研究を重ねた結果、表面の一部の領域に離型層を有し、前記離型層を有しない表面の残部の領域に、熱硬化性樹脂層を有する化粧板の構成とすることで、上記目的を達成できることを見出し、本発明を完成するに至った。   As a result of extensive research, the present inventors have a release layer in a partial area of the surface, and a decorative board having a thermosetting resin layer in the remaining area of the surface without the release layer. It was found that the above-described object can be achieved by adopting the structure, and the present invention has been completed.

即ち、本発明は、下記の化粧板に関する。
1.表面の一部の領域に離型層を有し、前記離型層を有しない表面の残部の領域に、熱硬化性樹脂層を有する、ことを特徴とする化粧板。
2.前記熱硬化性樹脂層は、メラミン樹脂を含有する、項1に記載の化粧板。
3.前記離型層は、硬化性樹脂を含有する、項1又は2に記載の化粧板。
4.前記硬化性樹脂は、電離放射線硬化型樹脂である、項3に記載の化粧板。
5.前記電離放射線硬化型樹脂は、重量平均分子量が500以上である、項4に記載の化粧板。
6.多孔質基材の表面の一部の領域に前記離型層を有し、前記離型層有しない、前記多孔質基材の表面の残部の領域に、前記熱硬化性樹脂層を有する、項1〜5のいずれかに記載の化粧板。
7.前記多孔質基材と、前記熱硬化性樹脂層及び/又は前記離型層との間に、更に、絵柄模様層を有する、項6に記載の化粧板。
8.前記多孔質基材の、前記熱硬化性樹脂層及び前記離型層を有する側とは反対側の面に、フェノール樹脂含浸紙を有する、項6又は7に記載の化粧板。
That is, this invention relates to the following decorative board.
1. A decorative board having a release layer in a partial region of the surface and a thermosetting resin layer in a remaining region of the surface not having the release layer.
2. Item 2. The decorative board according to Item 1, wherein the thermosetting resin layer contains a melamine resin.
3. Item 3. The decorative board according to Item 1 or 2, wherein the release layer contains a curable resin.
4). Item 4. The decorative board according to Item 3, wherein the curable resin is an ionizing radiation curable resin.
5. Item 5. The decorative board according to Item 4, wherein the ionizing radiation curable resin has a weight average molecular weight of 500 or more.
6). Item having the release layer in a partial region of the surface of the porous substrate and not having the release layer, and having the thermosetting resin layer in the remaining region of the surface of the porous substrate. The decorative board in any one of 1-5.
7). Item 7. The decorative board according to item 6, further comprising a pattern layer between the porous substrate and the thermosetting resin layer and / or the release layer.
8). Item 8. The decorative board according to Item 6 or 7, wherein a phenol resin-impregnated paper is provided on a surface of the porous substrate opposite to the side having the thermosetting resin layer and the release layer.

本発明の化粧板は、表面の一部の領域に離型層を有し、離型層を有しない表面の残部の領域に、熱硬化性樹脂層を有するので、熱硬化性樹脂層と離型層とが異なる意匠感を示すことにより、化粧板表面が鮮明なグロスマット調の意匠感を表現することができる。   The decorative board of the present invention has a release layer in a partial area of the surface and a thermosetting resin layer in the remaining area of the surface that does not have a release layer. Therefore, the decorative board is separated from the thermosetting resin layer. By showing a design feeling different from the mold layer, it is possible to express a glossy matte design feeling with a clear decorative board surface.

また、上記構成を備える本発明の化粧板は、表面の一部の領域に離型層を設け、熱硬化性樹脂を含浸させて加熱し、離型層を被覆している熱硬化した樹脂膜を剥離することにより製造することができるので、容易に製造することができる。   Further, the decorative board of the present invention having the above-described configuration is provided with a release layer in a partial region of the surface, impregnated with a thermosetting resin, heated, and coated with the release layer. Since it can manufacture by peeling off, it can manufacture easily.

本発明の化粧板の層構成の一例を模式的に示す断面図である。It is sectional drawing which shows typically an example of the laminated constitution of the decorative board of this invention. 本発明の化粧板を製造する製造方法において、工程1終了後の状態の一例を示す断面図である。In the manufacturing method which manufactures the decorative board of this invention, it is sectional drawing which shows an example of the state after process 1 completion | finish. 本発明の化粧板を製造する製造方法において、工程2終了後の状態の一例を示す断面図である。In the manufacturing method which manufactures the decorative board of this invention, it is sectional drawing which shows an example of the state after process 2 completion | finish.

本発明の化粧板は、表面の一部の領域に離型層を有し、上記離型層を有しない表面の残部の領域に、熱硬化性樹脂層を有する化粧板である。即ち、本発明の化粧板は、表面の一部の領域に離型層が形成されており、上記離型層が形成されていない表面の残部の領域には、熱硬化性樹脂層が形成されている。   The decorative board of the present invention is a decorative board having a release layer in a partial area of the surface and a thermosetting resin layer in the remaining area of the surface not having the release layer. That is, in the decorative board of the present invention, a release layer is formed in a part of the surface, and a thermosetting resin layer is formed in the remaining part of the surface where the release layer is not formed. ing.

以下、本発明の化粧板について説明する。なお、本発明において、表面とは、いわゆる「おもて面」であり、本発明の化粧板がフェノール樹脂含浸紙又は木質基材等に積層されて用いられる際に、フェノール樹脂含浸紙等と接触する面とは反対側の面であり、積層後に視認される面である。また、本明細書では、上記表面の方向を「おもて」又は「上」と称し、その反対側を「裏」又は「下」と称する場合がある。   Hereinafter, the decorative board of the present invention will be described. In the present invention, the surface is a so-called “front surface”, and when the decorative board of the present invention is used by being laminated on a phenol resin-impregnated paper or a wooden substrate, It is a surface on the opposite side to the surface to be contacted, and is a surface that is visually recognized after lamination. In the present specification, the direction of the surface may be referred to as “front” or “upper”, and the opposite side may be referred to as “back” or “lower”.

図1は、本発明の化粧板の層構成の一例を模式的に示す断面図である。図1において、本発明の化粧板は、熱硬化性樹脂が含浸され、熱硬化した多孔質基材1上に、離型層2及び熱硬化性樹脂層3が形成されている。このような層構成であることにより、図1に示す本発明の化粧板は、その表面の一部の領域に離型層2が形成されており、上記離型層2が形成されていない表面の残部の領域には、熱硬化性樹脂層3が形成されている。   FIG. 1 is a cross-sectional view schematically showing an example of the layer structure of the decorative board of the present invention. In FIG. 1, the decorative board of the present invention is impregnated with a thermosetting resin, and a release layer 2 and a thermosetting resin layer 3 are formed on a thermosetting porous substrate 1. Due to such a layer structure, the decorative board of the present invention shown in FIG. 1 has a surface in which the release layer 2 is formed in a partial region of the surface and the release layer 2 is not formed. The thermosetting resin layer 3 is formed in the remaining region.

図1に例示される本発明の化粧板は、上記構成であることにより、熱硬化性樹脂層3がグロスの意匠感を示し、離型層2がマットの意匠感を示すか、又は、熱硬化性樹脂層3がマットの意匠感を示し、離型層2がグロスの意匠感を示すことにより、化粧板表面が鮮明なグロスマット調の意匠感を表現することができる。また、上記構成を備える図1の本発明の化粧板は、多孔質基材1の表面の一部の領域に離型層2を設け、多孔質基材1に熱硬化性樹脂を含浸させて加熱し、離型層2を被覆している熱硬化した樹脂膜を剥離することにより製造することができるので、容易に製造することができる。   The decorative board of the present invention illustrated in FIG. 1 has the above-described configuration, so that the thermosetting resin layer 3 exhibits a glossy design feeling and the release layer 2 exhibits a mat design feeling, or heat When the curable resin layer 3 shows a mat design feeling and the release layer 2 shows a glossy design feeling, the decorative surface of the decorative board can have a clear gloss matte design feeling. Further, the decorative board of the present invention of FIG. 1 having the above configuration is provided with a release layer 2 in a partial region of the surface of the porous substrate 1, and the porous substrate 1 is impregnated with a thermosetting resin. Since it can manufacture by peeling off the thermosetting resin film which has heated and coat | covered the release layer 2, it can manufacture easily.

本発明の化粧板の表面における熱硬化性樹脂層が形成されている領域の面積(Sa)と、離型層が形成されている領域の面積(Sb)との面積比(Sa):(Sb)は、3:7〜9:1が好ましく、5:5〜8:2がより好ましい。面積比(Sa):(Sb)が上述の範囲内であると、本発明の化粧板が表現するグロスマット調の意匠が、より鮮明となる。   Area ratio (Sa) of the area (Sa) of the region where the thermosetting resin layer is formed on the surface of the decorative board of the present invention and the area (Sb) of the region where the release layer is formed: (Sb ) Is preferably 3: 7 to 9: 1, more preferably 5: 5 to 8: 2. When the area ratio (Sa) :( Sb) is within the above range, the gloss matte design expressed by the decorative board of the present invention becomes clearer.

熱硬化性樹脂層と離型層との高低差は、1〜50μmが好ましく、2〜30μmがより好ましい。上記高低差が上述の範囲内であると、本発明の化粧板が表現するグロスマット調の意匠が、より鮮明となる。   The height difference between the thermosetting resin layer and the release layer is preferably 1 to 50 μm, and more preferably 2 to 30 μm. When the height difference is within the above range, the gloss matte design expressed by the decorative board of the present invention becomes clearer.

以下、本発明の化粧板の層構成について説明する。本発明の化粧板は、上述のように表面の一部の領域に離型層が形成されており、離型層が形成されていない表面の残部の領域には、熱硬化性樹脂層が形成されていれば、その具体的構成(層構成)については限定されない。例えば、本発明の化粧板が多孔質基材を備える場合、多孔質基材の表面の一部の領域に離型層が形成されており、離型層が形成されていない、多孔質基材の表面の残部の領域には、熱硬化性樹脂層が形成されている構成が挙げられる。   Hereinafter, the layer structure of the decorative board of the present invention will be described. In the decorative board of the present invention, the release layer is formed in a part of the surface as described above, and the thermosetting resin layer is formed in the remaining part of the surface where the release layer is not formed. If it is, the specific configuration (layer configuration) is not limited. For example, when the decorative board of the present invention includes a porous substrate, the release layer is formed in a partial region of the surface of the porous substrate, and the release layer is not formed. In the remaining area of the surface, a configuration in which a thermosetting resin layer is formed may be mentioned.

以下、かかる層構成の化粧板を代表例として、各層について具体的に説明する。   Hereinafter, each layer will be specifically described with the decorative board having such a layer configuration as a representative example.

(離型層)
離型層は、本発明の化粧板の表面の一部の領域に形成される。上記離型層は、後述する本発明の化粧板の製造工程において、熱硬化性樹脂層を形成する際に、離型層の表面に一旦形成される熱硬化性樹脂の樹脂膜に対して離型性を有していれば特に限定されない。離型層は、例えば、多孔質基材等の表面に離型インキを塗布して硬化させることにより形成することができる。
(Release layer)
The release layer is formed in a partial region of the surface of the decorative board of the present invention. The release layer is separated from the thermosetting resin resin film once formed on the surface of the release layer when the thermosetting resin layer is formed in the manufacturing process of the decorative board of the present invention described later. If it has a moldability, it will not specifically limit. The release layer can be formed, for example, by applying release ink to the surface of a porous substrate or the like and curing it.

離型インキを構成する樹脂は、熱硬化性樹脂、電離放射線硬化型樹脂(例えば、電子線硬化型樹脂)等の硬化性樹脂;熱可塑性樹脂を用いることができるが、硬化性樹脂を用いることが好ましい。特に、高い表面硬度による耐傷性、凸形状保持性、生産性等の観点から、離型インキは電離放射線硬化型樹脂を含むことが好ましく、離型インキを構成する樹脂が電離放射線硬化型樹脂であることがより好ましい。   As the resin constituting the release ink, a curable resin such as a thermosetting resin or an ionizing radiation curable resin (for example, an electron beam curable resin); a thermoplastic resin can be used, but a curable resin should be used. Is preferred. In particular, from the viewpoint of scratch resistance due to high surface hardness, convex shape retention, productivity, etc., the release ink preferably contains an ionizing radiation curable resin, and the resin constituting the release ink is an ionizing radiation curable resin. More preferably.

熱硬化性樹脂としては、例えば、不飽和ポリエステル樹脂、ポリウレタン樹脂(2液硬化型ポリウレタンも含む)、エポキシ樹脂、アミノアルキッド樹脂、フェノール樹脂、尿素樹脂、ジアリルフタレート樹脂、メラミン樹脂、グアナミン樹脂、メラミン−尿素共縮合樹脂、珪素樹脂、ポリシロキサン樹脂等が挙げられる。   Examples of thermosetting resins include unsaturated polyester resins, polyurethane resins (including two-component curable polyurethanes), epoxy resins, amino alkyd resins, phenol resins, urea resins, diallyl phthalate resins, melamine resins, guanamine resins, and melamines. -Urea co-condensation resin, silicon resin, polysiloxane resin and the like.

上記樹脂には、架橋剤、重合開始剤等の硬化剤、重合促進剤を添加することができる。例えば、硬化剤としてはイソシアネート、有機スルホン酸塩等が不飽和ポリエステル樹脂やポリウレタン樹脂等に添加でき、有機アミン等がエポキシ樹脂に添加でき、メチルエチルケトンパーオキサイド等の過酸化物、アゾイソブチルニトリル等のラジカル開始剤が不飽和ポリエステル樹脂に添加することができる。   A curing agent such as a crosslinking agent and a polymerization initiator, and a polymerization accelerator can be added to the resin. For example, as curing agents, isocyanates, organic sulfonates, etc. can be added to unsaturated polyester resins, polyurethane resins, etc., organic amines, etc. can be added to epoxy resins, peroxides such as methyl ethyl ketone peroxide, azoisobutyl nitrile, etc. A radical initiator can be added to the unsaturated polyester resin.

熱硬化性樹脂を含む離型インキを用いて離型層を形成する方法は、例えば、熱硬化性樹脂の溶液をロールコート法、グラビアコート法等の塗布法で多孔質基材上に塗布し、乾燥及び硬化させる方法が挙げられる。   A method for forming a release layer using a release ink containing a thermosetting resin is, for example, by applying a solution of a thermosetting resin on a porous substrate by a coating method such as a roll coating method or a gravure coating method. And a method of drying and curing.

電離放射線硬化型樹脂は、電離放射線の照射により架橋重合反応を生じ、3次元の高分子構造に変化する樹脂であれば限定されない。例えば、電離放射線の照射により架橋可能な重合性不飽和結合又はエポキシ基を分子中に有するプレポリマー、オリゴマー及びモノマーの1種以上を使用することができる。中でも、多官能モノマー及びオリゴマーの1種以上を使用することが好ましい。上記電離放射線硬化型樹脂としては、例えば、ウレタンアクリレート、ポリエステルアクリレート、エポキシアクリレート等のアクリレート樹脂;シロキサン等のケイ素樹脂;ポリエステル樹脂;エポキシ樹脂などが挙げられる。   The ionizing radiation curable resin is not limited as long as it is a resin that undergoes a crosslinking polymerization reaction upon irradiation with ionizing radiation and changes to a three-dimensional polymer structure. For example, one or more of prepolymers, oligomers, and monomers having a polymerizable unsaturated bond or epoxy group that can be cross-linked by irradiation with ionizing radiation in the molecule can be used. Especially, it is preferable to use 1 or more types of a polyfunctional monomer and an oligomer. Examples of the ionizing radiation curable resin include acrylate resins such as urethane acrylate, polyester acrylate, and epoxy acrylate; silicon resins such as siloxane; polyester resins; and epoxy resins.

電離放射線硬化型樹脂の重量平均分子量は、500以上が好ましく、1000以上がより好ましい。電離放射線硬化型樹脂の重量平均分子量を上記範囲とすることで、上述のように多孔質基材等の表面に離型インキを塗布して硬化させることにより離型層を形成する際に、離型インキの多孔質基材等への浸み込みが抑制され、より確実に離型層を形成することができる。   The weight average molecular weight of the ionizing radiation curable resin is preferably 500 or more, and more preferably 1000 or more. By setting the weight average molecular weight of the ionizing radiation curable resin within the above range, the release layer is formed when the release layer is formed by applying and releasing the release ink on the surface of the porous substrate as described above. The penetration of the mold ink into the porous substrate or the like is suppressed, and the release layer can be formed more reliably.

電離放射線硬化型樹脂の重量平均分子量は、80000以下が好ましく、50000以下がより好ましい。電離放射線硬化型樹脂の重量平均分子量を上記範囲とすることで、上述のように多孔質基材等の表面に離型インキを塗布して硬化させることにより離型層を形成する際に、離型インキの粘度の上昇を抑制でき、離型インキの塗布が困難となり難い。   The weight average molecular weight of the ionizing radiation curable resin is preferably 80000 or less, and more preferably 50000 or less. By setting the weight average molecular weight of the ionizing radiation curable resin within the above range, the release layer is formed when the release layer is formed by applying and releasing the release ink on the surface of the porous substrate as described above. The increase in the viscosity of the mold ink can be suppressed, and it is difficult to apply the release ink.

なお、本明細書において、重量平均分子量は、ゲル浸透クロマトグラフィー(GPC)法により、ポリスチレンを標準物質に用いて測定される値である。   In this specification, the weight average molecular weight is a value measured using polystyrene as a standard substance by gel permeation chromatography (GPC).

電離放射線硬化型樹脂としては、重量平均分子量が500以上である多官能モノマー及びオリゴマーから選択される少なくとも1種が好ましい。このような多官能モノマー又はオリゴマーとしては、例えば、ジペンタエリスリトールヘキサアクリレート、ジペンタエリスリトールペンタアクリレート、ウレタンアクリレート、ポリエステルアクリレート、エポキシアクリレート等のアクリレート樹脂が挙げられる。   The ionizing radiation curable resin is preferably at least one selected from polyfunctional monomers and oligomers having a weight average molecular weight of 500 or more. Examples of such polyfunctional monomers or oligomers include acrylate resins such as dipentaerythritol hexaacrylate, dipentaerythritol pentaacrylate, urethane acrylate, polyester acrylate, and epoxy acrylate.

電離放射線としては、可視光線、紫外線(近紫外線、真空紫外線等)、X線、電子線、イオン線等があるが、この中でも、紫外線及び/又は電子線が望ましい。   Examples of the ionizing radiation include visible light, ultraviolet light (near ultraviolet light, vacuum ultraviolet light, etc.), X-rays, electron beams, ion beams, etc. Among them, ultraviolet light and / or electron beams are desirable.

紫外線源としては、超高圧水銀灯、高圧水銀灯、低圧水銀灯、カーボンアーク灯、ブラックライト蛍光灯、メタルハライドランプ灯の光源が使用できる。紫外線の波長としては、190〜380nm程度である。   As the ultraviolet light source, a light source such as an ultra-high pressure mercury lamp, a high pressure mercury lamp, a low pressure mercury lamp, a carbon arc lamp, a black light fluorescent lamp, or a metal halide lamp can be used. The wavelength of ultraviolet light is about 190 to 380 nm.

電子線源としては、例えば、コッククロフトワルト型、バンデグラフト型、共振変圧器型、絶縁コア変圧器型、直線型、ダイナミトロン型、高周波型等の各種電子線加速器が使用できる。電子線のエネルギーとしては、100〜1000keV程度が好ましく、100〜300keV程度がより好ましい。電子線の照射量は、2〜15Mrad程度が好ましい。   As the electron beam source, various electron beam accelerators such as a cockcroft-wald type, a bandegraft type, a resonant transformer type, an insulating core transformer type, a linear type, a dynamitron type, and a high frequency type can be used. The energy of the electron beam is preferably about 100 to 1000 keV, more preferably about 100 to 300 keV. The irradiation amount of the electron beam is preferably about 2 to 15 Mrad.

電離放射線硬化型樹脂は電子線を照射すれば十分に硬化するが、紫外線を照射して硬化させる場合には、光重合開始剤(増感剤)を添加することが好ましい。   The ionizing radiation curable resin is sufficiently cured when irradiated with an electron beam, but it is preferable to add a photopolymerization initiator (sensitizer) when it is cured by irradiation with ultraviolet rays.

ラジカル重合性不飽和基を有する樹脂系の場合の光重合開始剤は、例えば、アセトフェノン類、ベンゾフェノン類、チオキサントン類、ベンゾイン、ベンゾインメチルエーテル、ミヒラーベンゾイルベンゾエート、ミヒラーケトン、ジフェニルサルファイド、ジベンジルジサルファイド、ジエチルオキサイト、トリフェニルビイミダゾール、イソプロピル−N,N−ジメチルアミノベンゾエート等の少なくとも1種を使用することができる。また、カチオン重合性官能基を有する樹脂系の場合は、例えば、芳香族ジアゾニウム塩、芳香族スルホニウム塩、メタロセン化合物、ベンゾインスルホン酸エステル、フリールオキシスルホキソニウムジアリルヨードシル塩等の少なくとも1種を使用することができる。   Photopolymerization initiators in the case of resin systems having radically polymerizable unsaturated groups include, for example, acetophenones, benzophenones, thioxanthones, benzoin, benzoin methyl ether, Michler benzoylbenzoate, Michler ketone, diphenyl sulfide, dibenzyl disulfide , Diethyl oxide, triphenylbiimidazole, isopropyl-N, N-dimethylaminobenzoate and the like can be used. In the case of a resin system having a cationic polymerizable functional group, for example, at least one kind such as an aromatic diazonium salt, an aromatic sulfonium salt, a metallocene compound, a benzoin sulfonic acid ester, and a freeloxysulfoxonium diallyl iodosyl salt. Can be used.

光重合開始剤の添加量は特に限定されないが、一般に電離放射線硬化型樹脂100質量部に対して0.1〜10質量部程度である。   Although the addition amount of a photoinitiator is not specifically limited, Generally it is about 0.1-10 mass parts with respect to 100 mass parts of ionizing radiation curable resins.

電離放射線硬化型樹脂としては、耐熱性及び架橋密度を上げるため、多官能の重合性モノマーを含有することが好ましい。   The ionizing radiation curable resin preferably contains a polyfunctional polymerizable monomer in order to increase heat resistance and crosslinking density.

離型インキには、さらに離型性を付与する目的で、シリコーンオイルを含有させることが好ましい。シリコーンオイルとして、反応性シリコーンオイル、非反応性シリコーンオイル等を挙げることができる。   The release ink preferably contains silicone oil for the purpose of imparting releasability. Examples of the silicone oil include reactive silicone oil and non-reactive silicone oil.

反応性シリコーンオイルとは、側鎖又は末端に有機基を導入した変性シリコーンオイルのうち、導入する有機基の性質によって反応性を有するものをいう。反応性シリコーンオイルとして、具体的には、変性シリコーンオイル側鎖型、変性シリコーンオイル両末端型、変性シリコーンオイル片末端型、変性シリコーンオイル側鎖両末端型等において、導入する有機基がアミノ変性、エポキシ変性、メルカプト変性、カルボキシル変性、カルビノール変性、フェノール変性、メタクリル変性、異種官能基変性等であるものが挙げられる。これらの反応性シリコーンオイルは、単独で又は2種以上を混合して使用することができる。   The reactive silicone oil refers to a modified silicone oil having an organic group introduced into the side chain or terminal and having reactivity depending on the nature of the organic group to be introduced. As the reactive silicone oil, specifically, in the modified silicone oil side chain type, modified silicone oil both end type, modified silicone oil one end type, modified silicone oil side chain both end type, etc., the organic group to be introduced is amino-modified. , Epoxy modification, mercapto modification, carboxyl modification, carbinol modification, phenol modification, methacryl modification, heterogeneous functional group modification, and the like. These reactive silicone oils can be used alone or in admixture of two or more.

非反応性シリコーンオイルは、アミノ基、エポキシ基、メルカプト基、カルボキシ基、ヒドロキシ基、(メタ)アクリロイル基、アリル基等の反応性官能基を有しないシリコーンオイルであれば特に制限はない。非反応性シリコーンオイルとして、例えば、ポリシロキサンからなるシリコーンオイルのほか、ポリエーテル変性シリコーンオイル、アラルキル変性シリコーンオイル、フロロアルキル変性シリコーンオイル、長鎖アルキル変性シリコーンオイル、高級脂肪酸エステル変性シリコーンオイル、高級脂肪酸アミド変性シリコーンオイル、フェニル変性シリコーンオイル等が挙げられる。これらの非反応性シリコーンオイルは、単独で又は2種以上を混合して使用することができる。   The non-reactive silicone oil is not particularly limited as long as it is a silicone oil having no reactive functional group such as amino group, epoxy group, mercapto group, carboxy group, hydroxy group, (meth) acryloyl group, and allyl group. Non-reactive silicone oils include, for example, silicone oils composed of polysiloxanes, polyether-modified silicone oils, aralkyl-modified silicone oils, fluoroalkyl-modified silicone oils, long-chain alkyl-modified silicone oils, higher fatty acid ester-modified silicone oils, and higher grades. Examples include fatty acid amide-modified silicone oil and phenyl-modified silicone oil. These non-reactive silicone oils can be used alone or in admixture of two or more.

上記反応性シリコーンオイル又は非反応性シリコーンオイルは、離型インキの硬化時に硬化性樹脂の表面に配向し、離型性を発現する。   The reactive silicone oil or non-reactive silicone oil is oriented on the surface of the curable resin when the release ink is cured, and exhibits releasability.

上記反応性シリコーンオイル又は非反応性シリコーンオイルの使用量は、離型インキを構成する樹脂100質量部あたり0.1〜50質量部程度であり、好ましくは0.5〜20質量部程度であり、より好ましくは3〜20質量部程度であり、更に好ましくは3〜10質量部程度である。反応性シリコーンオイル又は非反応性シリコーンオイルの使用量を上記範囲とすることにより、離型層と硬化された樹脂膜との離型性が十分となる。   The amount of the reactive silicone oil or non-reactive silicone oil used is about 0.1 to 50 parts by mass, preferably about 0.5 to 20 parts by mass, per 100 parts by mass of the resin constituting the release ink. More preferably, it is about 3-20 mass parts, More preferably, it is about 3-10 mass parts. By making the usage-amount of a reactive silicone oil or a non-reactive silicone oil into the said range, the mold release property of a mold release layer and the hardened resin film will become enough.

離型インキは、さらに体質顔料を含有することが好ましい。体質顔料を含有することによって、インキにチキソ性を付与することができ、版を用いて離型層を印刷する際に、インキの形状が維持される。体質顔料としては特に限定されず、例えば、シリカ、タルク、クレー、硫酸バリウム、炭酸バリウム、硫酸カルシウム、炭酸カルシウム、炭酸マグネシウム等が挙げられる。これらのうち、材料設計の自由度が高く、意匠性、白さ、及びインキとしての塗工安定性に優れた材料であるシリカが好ましく、特に微粉末のシリカが好ましい。   It is preferable that the release ink further contains an extender pigment. By containing the extender, thixotropy can be imparted to the ink, and the shape of the ink is maintained when the release layer is printed using a plate. The extender is not particularly limited, and examples thereof include silica, talc, clay, barium sulfate, barium carbonate, calcium sulfate, calcium carbonate, and magnesium carbonate. Among these, silica, which is a material having a high degree of freedom in material design and excellent in design properties, whiteness, and coating stability as an ink, is preferable, and fine powder silica is particularly preferable.

これらの体質顔料のインキにおける含有量は、離型インキを構成する樹脂100質量部あたり0.1〜20質量部程度であり、好ましくは0.5〜15質量部程度であり、より好ましくは2〜15質量部程度であり、更に好ましくは、5〜15質量部程度である。体質顔料の使用量を上記範囲とすることにより、インキに十分なチキソ性を付与することができるとともに、隆起形状及び微細凹凸面の発現を付与する効果が得られる。   The content of these extender pigments in the ink is about 0.1 to 20 parts by mass, preferably about 0.5 to 15 parts by mass, more preferably 2 per 100 parts by mass of the resin constituting the release ink. It is about -15 mass parts, More preferably, it is about 5-15 mass parts. By making the usage-amount of extender the said range, while being able to provide sufficient thixotropy to ink, the effect which provides the expression of a protruding shape and a fine uneven surface is acquired.

離型インキは、無色であってもよいし、着色されていてもよい。着色する場合には、後述する絵柄模様層で使用する着色剤と同様のものを使用することができる。   The release ink may be colorless or colored. When coloring, the thing similar to the coloring agent used with the pattern pattern layer mentioned later can be used.

離型インキは、粘度を調整する目的で溶媒を含有してもよい。溶媒としては、水;トルエン、キシレン等の炭化水素化合物;メタノール、エタノール、メチルグリコール等のアルコール化合物;アセトン、メチルエチルケトン等のケトン化合物;ギ酸メチル、酢酸エチル等のエステル化合物;N−メチルピロリドン、N,N−ジメチルホルムアミド等の含窒素化合物;テロラヒドロフラン、ジオキサン等のエーテル化合物;塩化メチレン、クロロホルム等のハロゲン化炭化水素化合物;ジメチルスルホキシド等が挙げられる。これらの溶媒は、1種単独で又は2種以上を混合して使用することができる。離型インキ中の溶媒の量は、インキの粘度に応じて適宜設定することができる。   The release ink may contain a solvent for the purpose of adjusting the viscosity. Solvents include water; hydrocarbon compounds such as toluene and xylene; alcohol compounds such as methanol, ethanol and methyl glycol; ketone compounds such as acetone and methyl ethyl ketone; ester compounds such as methyl formate and ethyl acetate; N-methylpyrrolidone, N , N-dimethylformamide and the like; ether compounds such as terahydrofuran and dioxane; halogenated hydrocarbon compounds such as methylene chloride and chloroform; dimethyl sulfoxide and the like. These solvent can be used individually by 1 type or in mixture of 2 or more types. The amount of the solvent in the release ink can be appropriately set according to the viscosity of the ink.

離型インキには、得られる所望物性に応じて、従来より公知の添加剤を配合することができる。添加剤として、例えば、紫外線吸収剤、赤外線吸収剤、光安定剤、重合禁止剤、架橋剤、帯電防止剤、酸化防止剤、レベリング剤、カップリング剤、可塑剤、消泡剤、充填剤、熱ラジカル発生剤、アルミキレート剤等が挙げられる。   In the release ink, conventionally known additives can be blended depending on the desired physical properties to be obtained. As additives, for example, ultraviolet absorbers, infrared absorbers, light stabilizers, polymerization inhibitors, crosslinking agents, antistatic agents, antioxidants, leveling agents, coupling agents, plasticizers, antifoaming agents, fillers, Examples include a thermal radical generator and an aluminum chelating agent.

離型層は、本発明の化粧板の表面に所望のパターンで形成するとよい。離型層を形成するパターンとしては、例えば、木目板導管、石板表面凹凸、布表面テクスチャア、梨地、砂目、ヘアライン、万線条溝、等が挙げられる。   The release layer may be formed in a desired pattern on the surface of the decorative board of the present invention. Examples of the pattern for forming the release layer include a wood grain plate conduit, a stone plate surface unevenness, a cloth surface texture, a satin texture, a grain texture, a hairline, and a multiline groove.

離型層の厚みは特に限定されず、塗工時の層厚は1〜100μm程度、乾燥後の層厚は0.1〜20μm程度である。   The thickness of the release layer is not particularly limited, and the layer thickness at the time of coating is about 1 to 100 μm, and the layer thickness after drying is about 0.1 to 20 μm.

(熱硬化性樹脂層)
熱硬化性樹脂層は、本発明の化粧板の表面の上記離型層が形成されていない残部の領域に形成される。なお、上記熱硬化性樹脂層は、離型層の一部を被覆していてもよい。離型層の面積の50%以上の部分が露出して、化粧板の表面から視認されていれば、グロスマット調の意匠感を示すことができる。
(Thermosetting resin layer)
A thermosetting resin layer is formed in the remaining area | region where the said release layer is not formed of the surface of the decorative board of this invention. The thermosetting resin layer may cover a part of the release layer. If a portion of 50% or more of the area of the release layer is exposed and visually recognized from the surface of the decorative board, a glossy matte design feeling can be exhibited.

熱硬化性樹脂層を形成するのに用いられる熱硬化性樹脂としては、従来より公知の熱硬化型の樹脂を広く使用することができる。熱硬化性樹脂として、例えば、不飽和ポリエステル樹脂、ポリウレタン樹脂(2液硬化型ポリウレタンも含む)、エポキシ樹脂、アミノアルキッド樹脂、フェノール樹脂、尿素樹脂、ジアリルフタレート樹脂、メラミン樹脂、グアナミン樹脂、メラミン−尿素共縮合樹脂、珪素樹脂、ポリシロキサン樹脂等が挙げられる。本発明においては、耐熱性及び耐汚染性があり、硬度が高いメラミン樹脂を使用することが好ましい。   As the thermosetting resin used for forming the thermosetting resin layer, conventionally known thermosetting resins can be widely used. Examples of thermosetting resins include unsaturated polyester resins, polyurethane resins (including two-component curable polyurethane), epoxy resins, amino alkyd resins, phenol resins, urea resins, diallyl phthalate resins, melamine resins, guanamine resins, and melamines. Examples include urea cocondensation resins, silicon resins, polysiloxane resins, and the like. In the present invention, it is preferable to use a melamine resin having heat resistance and stain resistance and high hardness.

上記熱硬化性樹脂には、架橋剤、重合開始剤等の硬化剤、重合促進剤等を添加することができる。例えば、硬化剤としてはイソシアネート、有機スルホン酸塩等が不飽和ポリエステル樹脂又はポリウレタン樹脂等に添加でき、有機アミン等がエポキシ樹脂に添加でき、メチルエチルケトンパーオキサイド等の過酸化物、アゾイソブチルニトリル等のラジカル開始剤が不飽和ポリエステル樹脂に添加できる。   A curing agent such as a crosslinking agent and a polymerization initiator, a polymerization accelerator, and the like can be added to the thermosetting resin. For example, as curing agents, isocyanates, organic sulfonates, etc. can be added to unsaturated polyester resins or polyurethane resins, organic amines, etc. can be added to epoxy resins, peroxides such as methyl ethyl ketone peroxide, azoisobutyl nitrile, etc. A radical initiator can be added to the unsaturated polyester resin.

上記熱硬化性樹脂層を形成する方法としては、例えば、本発明の化粧板が多孔質基材を有する場合、多孔質基材に上記の熱硬化性樹脂を含浸させる方法が挙げられる。含浸は、上記の熱硬化性樹脂を、1)多孔質基材の離型層側、すなわち図1の上側から供給する、2)多孔質基材の裏面側、すなわち図1の下側から供給する、又は3)上記の1)及び2)の両側から供給する、ことにより行うことができる。この方法は特に限定されず、例えば、熱硬化性樹脂を入れた浴槽に多孔質基材の離型層が形成されている面又はその反対の面から浸漬させる方法;キスコーター、コンマコーター等のコーターにより熱硬化性樹脂を多孔性基材の離型層が形成されている面、その反対の面、又はこれらの両面に塗布する方法;スプレー装置、シャワー装置等により熱硬化性樹脂を多孔性基材の離型層が形成されている面、その反対の面、又はこれらの両面に吹き付ける方法、等が挙げられる。   As a method of forming the thermosetting resin layer, for example, when the decorative board of the present invention has a porous base material, a method of impregnating the porous base material with the thermosetting resin may be mentioned. In the impregnation, the above thermosetting resin is supplied from 1) the release layer side of the porous substrate, that is, from the upper side of FIG. 1, and 2) supplied from the back side of the porous substrate, that is, from the lower side of FIG. Or 3) by supplying from both sides of 1) and 2) above. This method is not particularly limited. For example, a method of immersing from a surface on which a release layer of a porous substrate is formed in a bath containing a thermosetting resin or the opposite surface; a coater such as a kiss coater or a comma coater By applying the thermosetting resin to the surface of the porous substrate on which the release layer is formed, the opposite surface, or both of these surfaces; spraying the thermosetting resin with a spray device, a shower device, etc. Examples thereof include a surface on which a release layer of the material is formed, a surface opposite to the surface, or a method of spraying on both surfaces.

熱硬化性樹脂は多孔質基材中に含浸するが、離型層の中には含浸されずに離型層を被覆する。なお、上記熱硬化性樹脂は離型層の少なくとも一部を被覆していればよく、例えば、離型層が占める全面積の30%以上が熱硬化性樹脂により被覆されていればよい。離型層の全面積における熱硬化性樹脂の被覆割合は、50〜100%程度であることが好ましい。   The thermosetting resin is impregnated in the porous substrate, but is not impregnated in the release layer and covers the release layer. In addition, the said thermosetting resin should just coat | cover at least one part of a mold release layer, for example, 30% or more of the total area which a mold release layer occupies should just be coat | covered with the thermosetting resin. The covering ratio of the thermosetting resin in the entire area of the release layer is preferably about 50 to 100%.

熱硬化性樹脂を含浸させた多孔質基材を加熱して、熱硬化性樹脂を硬化させることにより、熱硬化性樹脂層を形成することができる。加熱温度及び加熱時間は、使用する熱硬化性樹脂の種類等により適宜調整する。例えば、イソシアネート硬化型不飽和ポリエステル樹脂、及びウレタン硬化型ポリウレタン樹脂の場合は40〜60℃程度で1〜5日間程度であり、ポリシロキサン樹脂の場合は80〜150℃程度で1〜30分間程度であり、メラミン樹脂の場合は90〜160℃程度で30秒間〜30分間程度である。熱硬化性樹脂を硬化させる際、必要であれば、圧力を加えてもよい。   A thermosetting resin layer can be formed by heating a porous substrate impregnated with a thermosetting resin to cure the thermosetting resin. The heating temperature and the heating time are appropriately adjusted depending on the type of thermosetting resin used. For example, in the case of an isocyanate curable unsaturated polyester resin and a urethane curable polyurethane resin, it is about 1 to 5 days at about 40 to 60 ° C., and in the case of a polysiloxane resin, about 1 to 30 minutes at about 80 to 150 ° C. In the case of a melamine resin, it is about 90 to 160 ° C. and about 30 seconds to 30 minutes. When curing the thermosetting resin, pressure may be applied if necessary.

多孔質基材における樹脂含浸率は、化粧板の目的とする性能、多孔質基材の厚み等に応じて適宜調整することができる。樹脂含浸率として、30〜200%程度が好ましく、50〜150%程度がより好ましい。なお、樹脂含浸率は下記式により算出される。
樹脂含浸率(質量%)=[(含浸後の多孔質基材重量−含浸前の多孔質基材重量)/含浸前の多孔質基材重量]×100
The resin impregnation rate in the porous substrate can be appropriately adjusted according to the intended performance of the decorative board, the thickness of the porous substrate, and the like. The resin impregnation rate is preferably about 30 to 200%, more preferably about 50 to 150%. The resin impregnation rate is calculated by the following formula.
Resin impregnation rate (mass%) = [(weight of porous substrate after impregnation−weight of porous substrate before impregnation) / weight of porous substrate before impregnation] × 100

熱硬化性樹脂層の厚みは特に限定されず、塗工時の多孔質基材と熱硬化性樹脂との厚みの合計は、50〜500μm程度が好ましく、乾燥後の多孔質基材と熱硬化性樹脂との厚みの合計は、50〜300μm程度が好ましい。   The thickness of the thermosetting resin layer is not particularly limited, and the total thickness of the porous base material and the thermosetting resin during coating is preferably about 50 to 500 μm, and the porous base material after drying and thermosetting The total thickness with the conductive resin is preferably about 50 to 300 μm.

(多孔質基材)
多孔質基材としては、熱硬化性樹脂層を形成するための熱硬化性樹脂が含浸できるものであれば、特に制限されない。このような多孔質基材として、浸透性のある繊維質基材が挙げられる。浸透性のある繊維質基材としては、紙、合成紙、不織布等のシート状のものを用いることができる。多孔質基材として用いられる紙としては、薄葉紙、クラフト紙、チタン紙、リンター紙、板紙、石膏ボード紙、紙にポリ塩化ビニル樹脂をゾル又はドライラミネートしたいわゆるビニル壁紙原反、上質紙、コート紙、パーチメント紙、和紙等が挙げられる。紙類似シートとしては、ガラス繊維、石綿、チタン酸カリウム繊維、アルミナ繊維、シリカ繊維、炭素繊維等の無機等繊維質のシート状のもの;ポリエステル、ビニロン、ポリエチレン、ポリプロピレン等の合成樹脂繊維からなる不織布又は織布等を使用することができる。これらの多孔質基材のうち、熱硬化性樹脂の含浸性の点で、チタン紙、薄葉紙、クラフト紙、コート紙、アート紙、硫酸紙、グラシン紙、パーチメント紙、パラフィン紙、和紙が好ましく、チタン紙がより好ましい。
(Porous substrate)
The porous substrate is not particularly limited as long as it can be impregnated with a thermosetting resin for forming a thermosetting resin layer. An example of such a porous substrate is a permeable fibrous substrate. As the fibrous base material having permeability, a sheet-like material such as paper, synthetic paper, and non-woven fabric can be used. Paper used as the porous substrate is thin paper, kraft paper, titanium paper, linter paper, paperboard, gypsum board paper, so-called vinyl wallpaper original fabric, high-quality paper, coated paper with sol or dry lamination of polyvinyl chloride resin on paper Examples include paper, parchment paper, and Japanese paper. The paper-like sheet is a sheet of inorganic fiber such as glass fiber, asbestos, potassium titanate fiber, alumina fiber, silica fiber, or carbon fiber; made of synthetic resin fiber such as polyester, vinylon, polyethylene, or polypropylene Nonwoven fabrics or woven fabrics can be used. Of these porous substrates, titanium paper, thin paper, kraft paper, coated paper, art paper, sulfate paper, glassine paper, parchment paper, paraffin paper, and Japanese paper are preferred in terms of impregnation with thermosetting resin. Titanium paper is more preferred.

多孔質基材は、着色されていてもよい。この場合は、多孔質基材の製造段階、例えば多孔質基材が紙であればその抄造段階で、着色材(顔料又は染料)を配合することにより着色することができる。着色材としては、例えば、二酸化チタン、カーボンブラック、酸化鉄等の無機顔料、フタロシアニンブルー等の有機顔料のほか、各種の染料も使用することができる。これらは、公知又は市販のものから1種又は2種以上を選ぶことができる。また、着色材の配合量も、所望の色合い等に応じて適宜設定すればよい。   The porous substrate may be colored. In this case, it can be colored by blending a coloring material (pigment or dye) at the production stage of the porous substrate, for example, at the papermaking stage if the porous substrate is paper. As the colorant, for example, inorganic pigments such as titanium dioxide, carbon black and iron oxide, organic pigments such as phthalocyanine blue, and various dyes can be used. These can be selected from one or more known or commercially available ones. Further, the blending amount of the colorant may be set as appropriate according to the desired hue.

多孔質基材には、必要に応じて、充填剤、艶消し剤、発泡剤、難燃剤、滑剤、帯電防止剤、酸化防止剤、紫外線吸収剤、光安定化剤等の各種の添加剤が含まれていてもよい。   Various additives such as a filler, a matting agent, a foaming agent, a flame retardant, a lubricant, an antistatic agent, an antioxidant, an ultraviolet absorber, and a light stabilizer are added to the porous substrate as necessary. It may be included.

多孔質基材の坪量は特に限定されず、40〜150g/m程度が好ましい。多孔質基材の厚みは、最終製品の用途、使用方法等により適宜設定できるが、一般には50〜170μmが好ましい。 The basis weight of the porous substrate is not particularly limited, and is preferably about 40 to 150 g / m 2 . The thickness of the porous substrate can be set as appropriate depending on the use of the final product, the method of use, etc., but generally it is preferably 50 to 170 μm.

多孔質基材は、必要に応じて、絵柄模様層等を形成するインキの密着性を高めるために表面(おもて面)にコロナ放電処理を施してもよい。コロナ放電処理の方法・条件は、公知の方法に従って実施すればよい。   If necessary, the porous substrate may be subjected to corona discharge treatment on the surface (front surface) in order to improve the adhesion of the ink for forming the pattern layer or the like. What is necessary is just to implement the method and conditions of a corona discharge process according to a well-known method.

(絵柄模様層)
本発明の化粧板には、必要に応じて、多孔質基材と、熱硬化性樹脂層及び/又は離型層との間に、更に、絵柄模様層が形成されていてもよい。
(Pattern pattern layer)
In the decorative board of the present invention, if necessary, a pattern layer may be further formed between the porous substrate and the thermosetting resin layer and / or the release layer.

多孔質基材上に絵柄模様層を形成する場合、絵柄模様層における絵柄の種類等は限定的ではない。例えば、木目模様、レザー模様、石目模様、砂目模様、タイル貼模様、煉瓦積模様、布目模様、幾何学図形、文字、記号、抽象模様等が挙げられる。   When the pattern layer is formed on the porous substrate, the type of pattern in the pattern layer is not limited. For example, a wood grain pattern, a leather pattern, a stone pattern, a grain pattern, a tiled pattern, a brickwork pattern, a cloth pattern, a geometric figure, a character, a symbol, an abstract pattern, and the like can be given.

絵柄模様層の形成方法は特に限定されず、例えば、公知の着色剤(染料又は顔料)を結着材樹脂とともに溶剤(又は分散媒)中に溶解(又は分散)して得られるインキを用いた印刷法により、基材シート表面に形成すればよい。インキとしては、シートのVOCを低減する観点からは水性組成物を用いることもできる。絵柄模様層を印刷等により設ける場合には、その前に、多孔質基材表面にベタ印刷層を設けることもできる。   The method for forming the pattern layer is not particularly limited. For example, an ink obtained by dissolving (or dispersing) a known colorant (dye or pigment) in a solvent (or dispersion medium) together with a binder resin is used. What is necessary is just to form on the base-material sheet | seat surface by the printing method. As the ink, an aqueous composition can be used from the viewpoint of reducing the VOC of the sheet. When the pattern layer is provided by printing or the like, a solid print layer can be provided on the surface of the porous substrate before that.

インキに使用する着色剤としては、例えば、カーボンブラック、チタン白、亜鉛華、弁柄、紺青、カドミウムレッド等の無機顔料;アゾ顔料、レーキ顔料、アントラキノン顔料、キナクリドン顔料、フタロシアニン顔料、イソインドリノン顔料、ジオキサジン顔料等の有機顔料;アルミニウム粉、ブロンズ粉等の金属粉顔料;酸化チタン被覆雲母、酸化塩化ビスマス等の真珠光沢顔料;蛍光顔料;夜光顔料等が挙げられる。これらの着色剤は、単独又は2種以上を混合して使用することができる。これらの着色剤は、シリカ等のフィラー、有機ビーズ等の体質顔料、中和剤、界面活性剤等とともに用いてもよい。   Examples of the colorant used in the ink include inorganic pigments such as carbon black, titanium white, zinc white, petal, bitumen, and cadmium red; azo pigments, lake pigments, anthraquinone pigments, quinacridone pigments, phthalocyanine pigments, and isoindolinones. Examples thereof include organic pigments such as pigments and dioxazine pigments; metal powder pigments such as aluminum powder and bronze powder; pearlescent pigments such as titanium oxide-coated mica and bismuth oxide chloride; fluorescent pigments; These colorants can be used alone or in admixture of two or more. These colorants may be used together with fillers such as silica, extender pigments such as organic beads, neutralizing agents, surfactants and the like.

結着材樹脂としては、親水性処理されたポリエステル系ウレタン樹脂のほか、ポリエステル、ポリアクリレート、ポリビニルアセテート、ポリブタジエン、ポリ塩化ビニル、塩素化ポリプロピレン、ポリエチレン、ポリスチレン、ポリスチレン−アクリレート共重合体、ロジン誘導体、スチレン−無水マレイン酸共重合体のアルコール付加物、セルロース系樹脂、カゼイン樹脂なども併用できる。より具体的には、例えば、ポリアクリルアミド系樹脂、ポリ(メタ)アクリル酸系樹脂、ポリエチレンオキシド系樹脂、ポリN−ビニルピロリドン系樹脂、水溶性ポリエステル系樹脂、水溶性ポリアミド系樹脂、水溶性アミノ系樹脂、水溶性フェノール系樹脂、その他の水溶性合成樹脂;ポリヌクレオチド、ポリペプチド、多糖類等の水溶性天然高分子;等も使用することができる。また、例えば、天然ゴム、合成ゴム、ポリ酢酸ビニル系樹脂、(メタ)アクリル系樹脂、ポリ塩化ビニル系樹脂、ポリウレタン−ポリアクリル系樹脂等が変性したものないし前記天然ゴム等の混合物、その他の樹脂を使用できる。上記結着材樹脂は、単独又は2種以上を組み合わせて用いることができる。   As binder resin, in addition to polyester urethane resin treated with hydrophilicity, polyester, polyacrylate, polyvinyl acetate, polybutadiene, polyvinyl chloride, chlorinated polypropylene, polyethylene, polystyrene, polystyrene-acrylate copolymer, rosin derivative Alcohol adducts of styrene-maleic anhydride copolymers, cellulose resins, casein resins, and the like can also be used in combination. More specifically, for example, polyacrylamide resins, poly (meth) acrylic resins, polyethylene oxide resins, poly N-vinyl pyrrolidone resins, water-soluble polyester resins, water-soluble polyamide resins, water-soluble amino acids. Also usable are water-based resins, water-soluble phenolic resins, other water-soluble synthetic resins; water-soluble natural polymers such as polynucleotides, polypeptides, polysaccharides, and the like. Also, for example, natural rubber, synthetic rubber, polyvinyl acetate resin, (meth) acrylic resin, polyvinyl chloride resin, polyurethane-polyacrylic resin, etc. modified or a mixture of the above natural rubber, etc. Resin can be used. The said binder resin can be used individually or in combination of 2 or more types.

溶剤(又は分散媒)としては、例えば、ヘキサン、ヘプタン、オクタン、トルエン、キシレン、エチルベンゼン、シクロヘキサン、メチルシクロヘキサン等の石油系有機溶剤;酢酸エチル、酢酸ブチル、酢酸−2−メトキシエチル、酢酸−2−エトキシエチル等のエステル系有機溶剤;メチルアルコール、エチルアルコール、ノルマルプロピルアルコール、イソプロピルアルコール、イソブチルアルコール、エチレングリコール、プロピレングリコール等のアルコール系有機溶剤;アセトン、メチルエチルケトン、メチルイソブチルケトン、シクロヘキサノン等のケトン系有機溶剤;ジエチルエーテル、ジオキサン、テトラヒドロフラン等のエーテル系有機溶剤;ジクロロメタン、四塩化炭素、トリクロロエチレン、テトラクロロエチレン等の塩素系有機溶剤;水等の無機溶剤等が挙げられる。これらの溶剤(又は分散媒)は、単独で又は2種以上を混合して使用することができる。   Examples of the solvent (or dispersion medium) include petroleum organic solvents such as hexane, heptane, octane, toluene, xylene, ethylbenzene, cyclohexane, and methylcyclohexane; ethyl acetate, butyl acetate, 2-methoxyethyl acetate, and acetic acid-2 -Ester-based organic solvents such as ethoxyethyl; alcohol-based organic solvents such as methyl alcohol, ethyl alcohol, normal propyl alcohol, isopropyl alcohol, isobutyl alcohol, ethylene glycol, propylene glycol; ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone Organic solvents; ether organic solvents such as diethyl ether, dioxane, tetrahydrofuran; dichloromethane, carbon tetrachloride, trichloroethylene, tetrachloroethylene, etc. Chlorinated organic solvents; inorganic solvents such as water. These solvents (or dispersion media) can be used alone or in admixture of two or more.

絵柄模様層の形成に用いる印刷法としては、例えば、グラビア印刷法、オフセット印刷法、スクリーン印刷法、フレキソ印刷法、静電印刷法、インクジェット印刷法等が挙げられる。また、全面ベタ状の絵柄模様層を形成する場合には、例えば、ロールコート法、ナイフコート法、エアーナイフコート法、ダイコート法、リップコート法、コンマコート法、キスコート法、フローコート法、ディップコート法等の各種コーティング法が挙げられる。その他、手描き法、墨流し法、写真法、転写法、レーザービーム描画法、電子ビーム描画法、金属等の部分蒸着法、エッチング法等を用いたり、他の形成方法と組み合わせて用いたりしてもよい。   Examples of the printing method used for forming the pattern layer include a gravure printing method, an offset printing method, a screen printing method, a flexographic printing method, an electrostatic printing method, and an inkjet printing method. When forming a solid pattern pattern layer, for example, roll coating method, knife coating method, air knife coating method, die coating method, lip coating method, comma coating method, kiss coating method, flow coating method, dip coating Various coating methods such as a coating method may be mentioned. In addition, the hand-drawn method, the ink-sink method, the photographic method, the transfer method, the laser beam drawing method, the electron beam drawing method, the metal partial evaporation method, the etching method, etc. may be used or combined with other forming methods. Good.

絵柄模様層の厚みは特に限定されず、製品特性に応じて適宜設定できるが、塗工時の層厚は1〜200μm程度が好ましく、乾燥後の層厚は0.1〜20μm程度が好ましい。   The thickness of the pattern layer is not particularly limited and can be appropriately set according to product characteristics. However, the layer thickness at the time of coating is preferably about 1 to 200 μm, and the layer thickness after drying is preferably about 0.1 to 20 μm.

(接着剤層)
多孔質基材又は絵柄模様層と、離型層及び熱硬化性樹脂層との密着性を高めるため、多孔質基材又は絵柄模様層の上に接着剤層を形成してもよい。接着剤層は、透明性接着剤層であることが好ましく、当該透明性接着剤層としては、無色透明、着色透明、半透明等のいずれも含む。
(Adhesive layer)
An adhesive layer may be formed on the porous substrate or the pattern layer in order to improve the adhesion between the porous substrate or the pattern layer and the release layer and the thermosetting resin layer. The adhesive layer is preferably a transparent adhesive layer, and the transparent adhesive layer includes any of colorless and transparent, colored and transparent, and translucent.

接着剤としては特に限定されず、化粧板の分野で公知の接着剤が使用できる。化粧板の分野で公知の接着剤としては、例えば、ポリアミド樹脂、アクリル樹脂、酢酸ビニル樹脂等の熱可塑性樹脂、ウレタン系樹脂等の熱硬化性樹脂等が挙げられる。これら接着剤は1種単独で又は2種以上を組み合わせて用いることができる。また、イソシアネートを硬化剤とする二液硬化型ポリウレタン樹脂又はポリエステル樹脂も適用し得る。   It does not specifically limit as an adhesive agent, A well-known adhesive agent can be used in the field of a decorative board. Examples of the adhesive known in the decorative board field include thermoplastic resins such as polyamide resin, acrylic resin and vinyl acetate resin, and thermosetting resins such as urethane resin. These adhesives can be used individually by 1 type or in combination of 2 or more types. Further, a two-component curable polyurethane resin or polyester resin using isocyanate as a curing agent can also be applied.

接着剤層の厚みは特に限定されないが、乾燥後の厚みが0.1〜30μm程度、好ましくは1〜20μm程度である。   Although the thickness of an adhesive bond layer is not specifically limited, The thickness after drying is about 0.1-30 micrometers, Preferably it is about 1-20 micrometers.

(フェノール樹脂含浸紙)
本発明の化粧板には、必要に応じて、フェノール樹脂含浸紙が積層されていてもよい。上記フェノール樹脂含浸紙は、多孔質基材の、熱硬化性樹脂層及び離型層が形成されている側とは反対側の面に積層するとよい。
(Phenolic resin impregnated paper)
The decorative board of the present invention may be laminated with a phenol resin-impregnated paper as necessary. The phenol resin-impregnated paper is preferably laminated on the surface of the porous substrate opposite to the side on which the thermosetting resin layer and the release layer are formed.

フェノール樹脂含浸紙とは、一般に、コア紙として坪量150〜250g/m程度のクラフト紙にフェノール樹脂を含浸率45〜60%程度となるように含浸し、100〜140℃程度で乾燥させることにより製造された紙である。フェノール樹脂含浸紙には、市販品を使用することができる。フェノール樹脂含浸紙を積層する際には、必要に応じて、多孔質基材の裏面にコロナ放電処理を施したり、公知のプライマー層を塗布することにより裏面プライマー層を形成したりしてもよい。 The phenol resin impregnated paper is generally impregnated with kraft paper having a basis weight of about 150 to 250 g / m 2 as a core paper so that the impregnation rate is about 45 to 60% and dried at about 100 to 140 ° C. It is a paper manufactured by this. A commercially available product can be used for the phenol resin-impregnated paper. When laminating phenol resin impregnated paper, if necessary, the back surface of the porous substrate may be subjected to corona discharge treatment, or a back surface primer layer may be formed by applying a known primer layer. .

(裏面プライマー層)
多孔質基材の裏面(絵柄模様層、又は、離型層及び熱硬化性樹脂層が積層される面と反対側の面)又はフェノール樹脂含浸紙の裏面(多孔質基材が積層される面と反対側の面)には、必要に応じて、裏面プライマー層を設けてもよい。裏面プライマー層を設けると、例えば、本発明の化粧板と被着材とを積層する際に効果的である。
(Back primer layer)
The back surface of the porous substrate (the surface opposite to the surface on which the pattern layer or the release layer and the thermosetting resin layer are laminated) or the back surface of the phenol resin-impregnated paper (the surface on which the porous substrate is laminated) A reverse primer layer may be provided on the opposite surface) as required. Providing the back primer layer is effective, for example, when laminating the decorative board of the present invention and the adherend.

裏面プライマー層は、公知のプライマー剤を多孔質基材又はフェノール樹脂含浸紙に塗布することにより形成できる。プライマー剤としては、例えば、アクリル変性ウレタン樹脂(アクリルウレタン系樹脂)等からなるウレタン樹脂系プライマー剤、ウレタン−セルロース系樹脂(例えば、ウレタンと硝化綿の混合物にヘキサメチレンジイソシアネートを添加してなる樹脂)からなるプライマー剤、アクリルとウレタンのブロック共重合体からなる樹脂系プライマー剤等が挙げられる。プライマー剤には、必要に応じて、添加剤を配合してもよい。添加剤としては、例えば、炭酸カルシウム、クレー等の充填剤、水酸化マグネシウム等の難燃剤、酸化防止剤、滑剤、発泡剤、紫外線吸収剤、光安定剤などが挙げられる。添加剤の配合量は、製品特性に応じて適宜設定できる。   The back primer layer can be formed by applying a known primer to a porous substrate or phenol resin impregnated paper. Examples of the primer agent include a urethane resin-based primer agent made of an acrylic-modified urethane resin (acrylic urethane-based resin), a urethane-cellulose resin (for example, a resin obtained by adding hexamethylene diisocyanate to a mixture of urethane and nitrified cotton) ), A resinous primer agent made of a block copolymer of acrylic and urethane, and the like. You may mix | blend an additive with a primer agent as needed. Examples of the additive include fillers such as calcium carbonate and clay, flame retardants such as magnesium hydroxide, antioxidants, lubricants, foaming agents, ultraviolet absorbers, and light stabilizers. The blending amount of the additive can be appropriately set according to the product characteristics.

プライマー剤の塗布量は特に限定されないが、通常0.1〜100g/m、好ましくは0.1〜50g/m程度である。 Although the application amount of the primer agent is not particularly limited, it is usually 0.1 to 100 g / m 2 , preferably about 0.1 to 50 g / m 2 .

裏面プライマー層の厚みは特に限定されないが、通常0.01〜10μm、好ましくは0.1〜1μm程度である。   Although the thickness of a back surface primer layer is not specifically limited, Usually, 0.01-10 micrometers, Preferably it is about 0.1-1 micrometer.

本発明の化粧板は、鮮明なグロスマット調の意匠感を表現することができ、意匠性の高い化粧板である。この化粧板は、所定の成形加工等を施し、各種用途に用いることができる。例えば、上記化粧板を木質基材上に積層し、壁、天井、床等の建築物の内装、家具又は弱電又はOA機器のキャビネット等に利用することができる。木質基材として、具体的には、杉、檜、欅、松、ラワン、チーク、メラピー等の各種素材から作られた突板、木材単板、木材合板、パーティクルボード、中密度繊維板(MDF)、チップボード、又はチップボードが積層された複合基材等が挙げられる。上記木質基材としては、木材合板、パーティクルボード、中密度繊維板(MDF)を用いることが好ましい。   The decorative board of the present invention can express a clear gloss matte design and is a decorative board with high design properties. The decorative board can be used for various purposes after being subjected to a predetermined molding process. For example, the decorative plate can be laminated on a wooden base material and used for interiors of buildings such as walls, ceilings, floors, furniture, cabinets for light electrical or OA equipment, and the like. Specific examples of wood base materials include veneer, wood veneer, wood plywood, particle board, and medium density fiberboard (MDF) made from various materials such as cedar, firewood, firewood, pine, lawan, teak, and melapie. , Chip boards, or composite substrates on which chip boards are laminated. It is preferable to use wood plywood, particle board, or medium density fiberboard (MDF) as the wood substrate.

(化粧板の製造方法)
本発明の化粧板の製造方法としては特に限定されないが、例えば、本発明の化粧板が多孔質基材を有する場合、下記工程1〜3を有する製造方法により製造することができる。(1)多孔質基材の表面の一部の領域に離型層を設ける工程1、
(2)上記多孔質基材に熱硬化性樹脂を含浸させるとともに上記熱硬化性樹脂により上記離型層を被覆した後、加熱することにより上記熱硬化性樹脂を熱硬化させる工程2、及び(3)離型層の上を被覆している領域の熱硬化した樹脂膜を剥離する工程3。
(Manufacturing method of decorative board)
Although it does not specifically limit as a manufacturing method of the decorative board of this invention, For example, when the decorative board of this invention has a porous base material, it can manufacture with the manufacturing method which has the following processes 1-3. (1) Step 1 of providing a release layer in a partial region of the surface of the porous substrate,
(2) Step 2 of impregnating the porous base material with a thermosetting resin and coating the release layer with the thermosetting resin, followed by heating to thermoset the thermosetting resin; 3) Step 3 for removing the thermosetting resin film in the region covering the release layer.

(工程1)
工程1は、多孔質基材の表面の一部の領域に離型層を設ける工程である。上記工程1において用いられる多孔質基材は、上述のものを用いることができる。また、多孔質基材の表面の一部の領域に離型層を設ける方法としては、上述の方法を用いることができる。
(Process 1)
Step 1 is a step of providing a release layer in a partial region of the surface of the porous substrate. The above-mentioned thing can be used for the porous base material used in the said process 1. FIG. Moreover, the above-mentioned method can be used as a method of providing a release layer in a partial region of the surface of the porous substrate.

上記工程1終了後の状態の一例を図2に示す。図2において、離型層2は、多孔質基材1’の表面の全体ではなく一部の領域に設けられている。工程1において離型層2を多孔質基材1’の表面の一部の領域に設けることにより、工程3において、離型層2の上部を被覆している樹脂膜3’を剥離することができ、これにより化粧板の表面の一部の領域に離型層を形成し、離型層が形成されていない表面の残部の領域に、熱硬化性樹脂層を形成することができ、且つ、化粧板表面に凹凸を形成することができる。   An example of the state after completion of Step 1 is shown in FIG. In FIG. 2, the release layer 2 is provided not in the whole surface of the porous substrate 1 'but in a part of the region. By providing the release layer 2 in a part of the surface of the porous substrate 1 ′ in the step 1, the resin film 3 ′ covering the upper part of the release layer 2 can be peeled in the step 3. It is possible to form a release layer in a partial area of the surface of the decorative board, and to form a thermosetting resin layer in a remaining area of the surface where the release layer is not formed, and Unevenness can be formed on the decorative plate surface.

(工程2)
工程2は、上記多孔質基材に熱硬化性樹脂を含浸させるとともに上記熱硬化性樹脂により上記離型層を被覆した後、加熱することにより上記熱硬化性樹脂を熱硬化させる工程である。上記工程2において用いられる熱硬化性樹脂は、上述のものを用いることができる。また、多孔質基材に熱硬化性樹脂を含浸させるとともに上記熱硬化性樹脂により上記離型層を被覆した後、加熱する方法としては、上述の方法を用いることができる。
(Process 2)
Step 2 is a step of impregnating the porous base material with a thermosetting resin and coating the release layer with the thermosetting resin, followed by heating to thermoset the thermosetting resin. The above-mentioned thing can be used for the thermosetting resin used in the above step 2. Moreover, the above-mentioned method can be used as a method of heating after impregnating the porous substrate with a thermosetting resin and coating the release layer with the thermosetting resin.

上記工程2終了後の状態の一例を図3に示す。図3において、含浸した熱硬化性樹脂が熱硬化した多孔質基材1上に、熱硬化性樹脂層3が形成されている。また、剥離層2上に、熱硬化性樹脂が熱硬化した樹脂膜3’が形成されている。   An example of the state after completion of step 2 is shown in FIG. In FIG. 3, a thermosetting resin layer 3 is formed on a porous substrate 1 obtained by thermosetting the impregnated thermosetting resin. Further, a resin film 3 ′ obtained by thermosetting a thermosetting resin is formed on the release layer 2.

(工程3)
工程3は、離型層の上を被覆している熱硬化した樹脂膜を剥離する工程である。離型層の上を被覆している熱硬化した樹脂膜を剥離する方法は特に限定されない。例えば、化粧板表面に、マスキングフィルム等の保護フィルムを貼り付け、その後に該フィルムを剥がす方法や、熱硬化した樹脂膜の表面をバフ研磨する方法等が挙げられる。
(Process 3)
Step 3 is a step of peeling off the thermosetting resin film covering the release layer. There is no particular limitation on the method for peeling the thermosetting resin film covering the release layer. For example, a method of sticking a protective film such as a masking film on the decorative plate surface, and then peeling the film, a method of buffing the surface of the thermosetting resin film, and the like can be mentioned.

離型層の上を被覆している熱硬化した樹脂膜を剥離する方法としては、また、当該樹脂膜をたわし、メラミンスポンジ、スチールウール等により研磨する方法;樹脂膜にセロテープ(登録商標)、ガムテープ(登録商標)等の粘着テープを貼り付け、剥離する方法;樹脂膜上に、予め溶剤に溶解させた塩化ゴム系樹脂、ウレタン樹脂、ポリエステル樹脂等の樹脂液を塗工し、乾燥した後剥離する方法;樹脂膜上に、ホットメルト接着剤を塗工した後に低温下で剥離する方法;樹脂膜に、樹脂板、金属板等を貼り付けた後剥離する方法;樹脂膜を、高圧洗浄機により洗浄して剥離する方法;粘着ゴムローラー、粘着ゴムシート等により樹脂膜を剥離する方法等が挙げられる。   As a method of peeling the thermosetting resin film covering the release layer, the method is also a method of rubbing the resin film and polishing it with melamine sponge, steel wool, etc .; cellotape (registered trademark) on the resin film, A method of applying and peeling an adhesive tape such as a gum tape (registered trademark); After applying a resin solution such as a chlorinated rubber resin, a urethane resin, or a polyester resin previously dissolved in a solvent on the resin film and drying it Method of peeling; Method of peeling at low temperature after applying hot melt adhesive on resin film; Method of peeling after attaching resin plate, metal plate, etc. to resin film; High pressure cleaning of resin film A method of cleaning and peeling with a machine; a method of peeling a resin film with an adhesive rubber roller, an adhesive rubber sheet or the like.

工程3により、図1に示す本発明の化粧板を得ることができる。離型層の上を被覆している熱硬化した樹脂膜を剥離することで、図1に示すように、離型層2が露出する。離型層2が存在しない箇所では、熱硬化性樹脂層3は、工程3によっても剥離されない。これにより、表面の一部の領域に離型層2が形成されており、離型層2が形成されていない表面の残部の領域には、熱硬化性樹脂層3が形成されている本発明の化粧板を得ることができる。   By the process 3, the decorative board of the present invention shown in FIG. 1 can be obtained. By releasing the thermosetting resin film covering the release layer, the release layer 2 is exposed as shown in FIG. In the place where the release layer 2 does not exist, the thermosetting resin layer 3 is not peeled off even by the step 3. Thereby, the mold release layer 2 is formed in a partial area of the surface, and the thermosetting resin layer 3 is formed in the remaining area of the surface where the mold release layer 2 is not formed. A decorative board can be obtained.

上述の方法により製造される本発明の化粧板は、表面の一部の領域に形成された離型層、及び離型層が形成されていない表面の残部の領域に形成された熱硬化性樹脂層により、鮮明なグロスマット調の意匠感を表現することができる。例えば、図1に示す化粧板では、熱硬化性樹脂層3がグロス調の意匠感を与え、離型層2がマット調の意匠感を与えることにより、鮮明なグロスマット調の意匠感を表現することができる。また、熱硬化性樹脂層3と、離型層2との高低差を大きくすることにより、グロスマット調の意匠感がより鮮明となる。   The decorative board of the present invention produced by the above-described method includes a release layer formed in a partial region of the surface, and a thermosetting resin formed in the remaining region of the surface where the release layer is not formed. The layer can express a clear gloss matte design feeling. For example, in the decorative board shown in FIG. 1, the thermosetting resin layer 3 gives a glossy design feeling and the release layer 2 gives a matte design feeling, thereby expressing a clear glossy matte design feeling. can do. Further, by increasing the difference in height between the thermosetting resin layer 3 and the release layer 2, the gloss matte design feel becomes clearer.

なお、上記工程3において、離型層の上に存在する熱硬化した樹脂膜のすべてが剥離される必要はなく、離型層の上に存在する熱硬化した樹脂膜の一部が残っていてもよい。離型層の面積の50%以上の部分が剥離されていれば、グロスマット調の意匠感を得ることができる。   In Step 3, it is not necessary that all of the thermosetting resin film existing on the release layer is peeled off, and a part of the thermosetting resin film existing on the release layer remains. Also good. If 50% or more of the area of the release layer is peeled off, a glossy matte design feeling can be obtained.

このように、多孔質基材上の一部に離型層を設け、熱硬化性樹脂を含浸させて加熱した後に離型層の上の熱硬化した樹脂膜を剥離することで、化粧板表面が鮮明なグロスマット調の意匠感を表現することができる。本発明の化粧板は、上記方法により製造することができるので、従来の方法において意匠の種類だけ必要であった表面処理した鏡面板が不要となるため、容易に製造することができ、コストを低くすることができる。さらに、多孔質基材の上に絵柄模様層を設ける場合、絵柄模様層及び離型層を印刷により作成することで、絵柄模様層の模様に同調させて離型層を印刷することが可能となる。これにより、従来の方法で困難であった下地の絵柄とグロスマット調の意匠とを同調させることが可能となり、より意匠性の高い化粧板を製造することができる。   As described above, the surface of the decorative board is provided by providing a release layer on a part of the porous substrate, impregnating the thermosetting resin, heating, and then peeling off the thermosetting resin film on the release layer. Can express a vivid gloss matte design. Since the decorative board of the present invention can be manufactured by the above-described method, a surface-finished mirror plate that is necessary only for the type of design in the conventional method is not necessary, so that it can be easily manufactured and the cost can be reduced. Can be lowered. Furthermore, when the pattern layer is provided on the porous substrate, it is possible to print the release layer in synchronization with the pattern of the pattern layer by creating the pattern layer and the release layer by printing. Become. As a result, it becomes possible to synchronize the background pattern and the gloss matte design, which was difficult with the conventional method, and it is possible to manufacture a decorative board with higher design.

以下に実施例及び比較例を示して本発明をより詳しく説明する。但し、本発明は実施例に限定されない。   Hereinafter, the present invention will be described in more detail with reference to Examples and Comparative Examples. However, the present invention is not limited to the examples.

実施例1
(1)離型インキの調製
電離放射線硬化性モノマー(東亞合成株式会社製、アロニックスM400)60質量部、反応性シリコーン(信越化学株式会社製、X−22−164B)0.6質量部、及びメチルエチルケトン(丸善石油化学株式会社)40質量部を、プロセスホモジナイザーPH91(株式会社エスエムテー製)を用いて、回転数2000rpmで1時間撹拌して離型インキを調製した。
Example 1
(1) Preparation of release ink Ionizing radiation curable monomer (Toagosei Co., Ltd., Aronix M400) 60 parts by mass, reactive silicone (Shin-Etsu Chemical Co., Ltd., X-22-164B) 0.6 parts by mass, and A release ink was prepared by stirring 40 parts by mass of methyl ethyl ketone (Maruzen Petrochemical Co., Ltd.) using a process homogenizer PH91 (manufactured by SMT Co., Ltd.) at a rotational speed of 2000 rpm for 1 hour.

(2)化粧板の製造
原紙として坪量100g/mの白チタン紙(KJ特殊紙株式会社製、KW−1002P)を使用し、絵柄印刷インキ(DICグラフィックス株式会社製、オーデSPTI)を用いて絵柄を印刷した後、上記(1)で製造した離型インキを用いて木目柄を印刷し、165kVの加速電圧にて5Mradの電子線照射を行い、離型層を形成した。離型層は、木目柄であるため、厚みが厚い箇所と薄い箇所とが存在しており、離型層の厚みは0.2〜3μmであった。
(2) Manufacture of decorative board Using white titanium paper (KJ Special Paper Co., Ltd., KW-1002P) with a basis weight of 100 g / m 2 as the base paper, design printing ink (DIC Graphics Co., Ltd., Ode SPTI) After printing the pattern, the wood grain pattern was printed using the release ink produced in (1) above, and irradiated with 5 Mrad of electron beam at an acceleration voltage of 165 kV to form a release layer. Since the release layer has a wood grain pattern, there are a thick portion and a thin portion, and the thickness of the release layer was 0.2 to 3 μm.

次いでメラミンホルムアルデヒド樹脂50質量部、水45質量部、及びイソプロピルアルコール5質量部からなる熱硬化性樹脂を、含浸用の含浸装置を用いてメラミン樹脂が100g/m(乾燥時)の割合となるように含浸し、乾燥することにより含浸化粧シートを得た。この含浸化粧シートを、クラフト紙にフェノール樹脂からなる樹脂液を含浸した、坪量245g/mのフェノール樹脂含浸コア紙(太田産業株式会社、太田コア)4枚の上に積層し、積層体を2枚の鏡面板で挟み、熱プレス機を用いて圧力100kg/cmで、成型温度150℃で10分間の条件にて加熱成型し、メラミン樹脂を含有する熱硬化性樹脂層を形成して、高圧メラミン化粧板の成型物を得た。この際、離型層上には、熱硬化した樹脂膜が形成された。 Next, a thermosetting resin composed of 50 parts by mass of melamine formaldehyde resin, 45 parts by mass of water, and 5 parts by mass of isopropyl alcohol is used at a rate of 100 g / m 2 (when dried) using an impregnation apparatus for impregnation. The impregnated decorative sheet was obtained by impregnation as described above and drying. This impregnated decorative sheet is laminated on four sheets of phenol resin-impregnated core paper (Ota Sangyo Co., Ltd., Ota Core) having a basis weight of 245 g / m 2 in which a kraft paper is impregnated with a resin solution comprising a phenol resin. Is sandwiched between two mirror plates and heat-molded using a hot press machine at a pressure of 100 kg / cm 2 and a molding temperature of 150 ° C. for 10 minutes to form a thermosetting resin layer containing a melamine resin. As a result, a molded article of a high-pressure melamine decorative board was obtained. At this time, a thermoset resin film was formed on the release layer.

次いで剥離工程として、高圧メラミン化粧板の表面にマスキングテープ(株式会社スミロン製:E−207)を貼付け、その後、貼付けたマスキングテープを剥がして、離型層上に形成された熱硬化した樹脂膜を剥離して、化粧板を製造した。得られた化粧板の熱硬化性樹脂層の厚みは30μmであり、離型層と熱硬化性樹脂層との高低差、すなわち、化粧板の表面高低差は5μmであった。   Next, as a peeling step, a masking tape (manufactured by Sumilon Co., Ltd .: E-207) is pasted on the surface of the high-pressure melamine decorative board, and then the pasted masking tape is peeled off to form a thermosetting resin film formed on the release layer. Was peeled off to produce a decorative board. The thickness of the thermosetting resin layer of the obtained decorative board was 30 μm, and the height difference between the release layer and the thermosetting resin layer, that is, the surface height difference of the decorative board was 5 μm.

実施例2〜21
離型インキの組成を表1のように変更した以外は実施例1と同様にして、化粧板を製造した。
Examples 2 to 21
A decorative board was produced in the same manner as in Example 1 except that the composition of the release ink was changed as shown in Table 1.

比較例1
木目柄を印刷しなかった以外は実施例1と同様にして、化粧板を製造した。
Comparative Example 1
A decorative board was produced in the same manner as in Example 1 except that the wood grain pattern was not printed.

実施例22〜37
離型インキを構成する樹脂として表3に示す樹脂を用い、表4に示すシリカ、表5に示すシリコーンを用いて離型インキの組成を表6及び7のように変更した以外は実施例1と同様にして、化粧板を製造した。
Examples 22-37
Example 1 except that the resin shown in Table 3 was used as the resin constituting the release ink, and the composition of the release ink was changed as shown in Tables 6 and 7 using silica shown in Table 4 and silicone shown in Table 5. In the same manner, a decorative board was produced.

実施例1〜37、及び比較例1の化粧板について、以下の測定方法により意匠感及び表面高低差を評価した。   About the decorative board of Examples 1-37 and the comparative example 1, the design feeling and the surface height difference were evaluated with the following measuring methods.

意匠感
化粧板の表面を目視により観察し、下記の評価基準に基づいて評価した。
◎:グロスマット感が十分に鮮明であり、良好
○:グロスマット感が鮮明であり、良好
△:グロスマット感が鮮明でないが、使用可能
×:グロスマット感が鮮明でなく、使用不可
Was visually observed the surface of the design sense veneer was evaluated based on the following evaluation criteria.
◎: Glossy matt feeling is sufficiently clear, good ◯: Glossy matt feeling is clear, good △: Glossy matt feeling is not clear but can be used ×: Glossy matt feeling is not clear and cannot be used

表面高低差
化粧板の表面高低差を、株式会社小坂研究所製 三次元表面粗さ測定器SE−30Kを使用して、JIS B 0601:2013に規定された方法に従って測定した。具体的には、化粧板表面の離型層が形成されていない領域(熱硬化性樹脂層が形成されている領域)と離型層が形成されている領域(熱硬化した樹脂膜が剥離した部分)との高低差を測定した。表面の最大高さ粗さ(Rz)を表面高低差のパラメ−タ−として用いた。10箇所の平均値を表1に記載した。
The surface height difference of the decorative sheet was measured using a three-dimensional surface roughness measuring instrument SE-30K manufactured by Kosaka Laboratory Ltd. according to the method defined in JIS B 0601: 2013. Specifically, the area where the release layer is not formed on the decorative board surface (area where the thermosetting resin layer is formed) and the area where the release layer is formed (the thermosetting resin film is peeled off) The height difference from the part) was measured. The maximum height roughness (Rz) of the surface was used as a parameter for the surface height difference. The average values at 10 locations are shown in Table 1.

結果を表1、2、6及び7に示す。   The results are shown in Tables 1, 2, 6 and 7.

Figure 2016182808
Figure 2016182808

Figure 2016182808
Figure 2016182808

Figure 2016182808
Figure 2016182808

Figure 2016182808
Figure 2016182808

Figure 2016182808
Figure 2016182808

Figure 2016182808
Figure 2016182808

Figure 2016182808
Figure 2016182808

1.熱硬化性樹脂が含浸及び熱硬化した多孔質基材
1’.多孔質基材
2.離型層
3.熱硬化性樹脂層
3’.熱硬化した樹脂膜
1. Porous substrate 1 '. Impregnated and thermoset with thermosetting resin. 1. porous substrate 2. Release layer Thermosetting resin layer 3 ′. Thermoset resin film

Claims (8)

表面の一部の領域に離型層を有し、前記離型層を有しない表面の残部の領域に、熱硬化性樹脂層を有する、ことを特徴とする化粧板。   A decorative board having a release layer in a partial region of the surface and a thermosetting resin layer in a remaining region of the surface not having the release layer. 前記熱硬化性樹脂層は、メラミン樹脂を含有する、請求項1に記載の化粧板。   The said thermosetting resin layer is a decorative board of Claim 1 containing a melamine resin. 前記離型層は、硬化性樹脂を含有する、請求項1又は2に記載の化粧板。   The decorative sheet according to claim 1, wherein the release layer contains a curable resin. 前記硬化性樹脂は、電離放射線硬化型樹脂である、請求項3に記載の化粧板。   The decorative board according to claim 3, wherein the curable resin is an ionizing radiation curable resin. 前記電離放射線硬化型樹脂は、重量平均分子量が500以上である、請求項4に記載の化粧板。   The decorative sheet according to claim 4, wherein the ionizing radiation curable resin has a weight average molecular weight of 500 or more. 多孔質基材の表面の一部の領域に前記離型層を有し、前記離型層有しない、前記多孔質基材の表面の残部の領域に、前記熱硬化性樹脂層を有する、請求項1〜5のいずれかに記載の化粧板。   Having the release layer in a partial region of the surface of the porous substrate, and not having the release layer, and having the thermosetting resin layer in the remaining region of the surface of the porous substrate, The decorative board in any one of claim | item 1 -5. 前記多孔質基材と、前記熱硬化性樹脂層及び/又は前記離型層との間に、更に、絵柄模様層を有する、請求項6に記載の化粧板。   The decorative board according to claim 6, further comprising a pattern layer between the porous substrate and the thermosetting resin layer and / or the release layer. 前記多孔質基材の、前記熱硬化性樹脂層及び前記離型層を有する側とは反対側の面に、フェノール樹脂含浸紙を有する、請求項6又は7に記載の化粧板。   The decorative board according to claim 6 or 7, wherein a phenol resin-impregnated paper is provided on a surface of the porous substrate opposite to the side having the thermosetting resin layer and the release layer.
JP2015181148A 2015-03-13 2015-09-14 Veneer Active JP6716877B2 (en)