JP2011085065A - Turbine device repairing method - Google Patents

Turbine device repairing method Download PDF

Info

Publication number
JP2011085065A
JP2011085065A JP2009238204A JP2009238204A JP2011085065A JP 2011085065 A JP2011085065 A JP 2011085065A JP 2009238204 A JP2009238204 A JP 2009238204A JP 2009238204 A JP2009238204 A JP 2009238204A JP 2011085065 A JP2011085065 A JP 2011085065A
Authority
JP
Japan
Prior art keywords
abnormal
joint surface
spraying
turbine apparatus
thermal spray
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
JP2009238204A
Other languages
Japanese (ja)
Other versions
JP5355343B2 (en
Inventor
Mitsuo Takahashi
光男 高橋
Masaki Murakami
雅規 村上
Toshiyuki Ohashi
俊之 大橋
Yutaka Sato
豊 佐藤
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Toshiba Corp
Toshiba Industrial Technology Corp
Original Assignee
Toshiba Corp
Toshiba Industrial Technology Corp
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Toshiba Corp, Toshiba Industrial Technology Corp filed Critical Toshiba Corp
Priority to JP2009238204A priority Critical patent/JP5355343B2/en
Publication of JP2011085065A publication Critical patent/JP2011085065A/en
Application granted granted Critical
Publication of JP5355343B2 publication Critical patent/JP5355343B2/en
Expired - Fee Related legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

<P>PROBLEM TO BE SOLVED: To efficiently repair a turbine device in a turbine device repairing method for repairing the internal casing portions or the like of the turbine device. <P>SOLUTION: This method for repairing the internal casing of the turbine device includes: an inspection step (Step S1) of detecting abnormal portions which are formed on the joint surfaces of the internal casing portions and which are deformed and recessed in a direction with the internal casing portions mutually separated other than a sound joint surface, and measuring the deformation volume of the abnormal portions; a foundation treatment step (Step S3) of setting the surfaces of the abnormal portions to a predetermined surface roughness; a thermal spray step (Step S4) of thermally spraying thermal spray material containing chromium alloy material to the abnormal portions so that a projecting portion projecting from the sound joint surface is formed; and a step (Step S5) of removing the projecting portion so that the surface position of a thermally sprayed portion is set to the same position as the sound joint surface. <P>COPYRIGHT: (C)2011,JPO&INPIT

Description

本発明は、タービン装置の内部車室部等の補修を行うためのタービン装置補修方法に関する。   The present invention relates to a turbine device repair method for repairing an internal casing or the like of a turbine device.

軸流蒸気タービン等のタービン装置は、一般に軸周りを回転するロータと、このロータの外側に配置されて蒸気流路等を形成するノズルと、このノズルを収容して固定する内部車室と、この内部車室を収容する外部車室と、を有する。この内部車室は、ノズルおよびロータの間に形成された所定の間隙を保持するように、ノズル等を固定している。また、内部車室は、シール機能を有する圧力容器でもある。この内部車室は、上半および下半に分割可能で、それぞれに分割面(接合面)が形成されている。   A turbine apparatus such as an axial flow steam turbine generally includes a rotor that rotates around an axis, a nozzle that is disposed outside the rotor to form a steam flow path, an internal casing that houses and fixes the nozzle, And an external compartment for housing the internal compartment. In this internal casing, nozzles and the like are fixed so as to maintain a predetermined gap formed between the nozzle and the rotor. The inner casing is also a pressure vessel having a sealing function. The internal casing can be divided into an upper half and a lower half, and a dividing surface (joint surface) is formed on each of them.

当該タービン装置を長期使用すると、ロータの損傷や内部車室の接合面の侵食等の不具合が起こることがある。ロータの補修については、例えば特許文献1に開示されているような方法が知られている。   When the turbine device is used for a long period of time, problems such as damage to the rotor and erosion of the joint surface of the inner casing may occur. For repairing the rotor, for example, a method as disclosed in Patent Document 1 is known.

一方、内部車室の接合面は、熱影響等により変形、流体(蒸気)等による侵食等が発生することがある。これにより、ノズルの固定位置の変化やシール機能の低下等の不具合が生じることがある。このような不具合が発生すると、回転しているロータがノズルに接触して発生する振動や、蒸気漏れ等のトラブルが発生する。このため、上記のような変形や侵食を補修する必要がある。   On the other hand, the joint surface of the internal compartment may be deformed due to thermal effects or the like, and may be eroded by fluid (steam) or the like. As a result, problems such as a change in the nozzle fixing position and a decrease in the sealing function may occur. When such a problem occurs, troubles such as vibration generated when the rotating rotor comes into contact with the nozzle and steam leakage occur. For this reason, it is necessary to repair the above deformation and erosion.

特開2004−256903号公報JP 2004-256903 A

従来の内部車室の補修は、先ずタービン装置を分解して、内部車室を補修するための専用の加工設備がある工場へ移送して、修理を行っていた。このため、移送のために長時間を必要としていた。また、従来の補修は、フライス加工等によって異常部位を削り込んで健全な面を形成して補修していた。この方法では、異常部位の他に、異常が発生していない健全な部分まで削り込む必要がある。このため、補修加工は長時間を必要としていた。   In the conventional internal casing repair, the turbine device is first disassembled and transferred to a factory having a dedicated processing facility for repairing the internal casing. For this reason, a long time is required for transfer. Further, in the conventional repair, the abnormal part is cut by milling or the like to form a healthy surface for repair. In this method, it is necessary to cut down to a healthy part where no abnormality has occurred in addition to the abnormal part. For this reason, the repair process required a long time.

本発明は上述した課題を解決するためになされたものであり、その目的は、タービン装置を効率よく補修することである。   The present invention has been made to solve the above-described problems, and an object thereof is to efficiently repair a turbine apparatus.

上記目的を達成するための本発明に係るタービン装置補修方法は、軸周りを回転するロータと、このロータの半径方向外側に配置されたノズルと、このノズルを半径方向外側から覆いながら固定可能で軸に平行な平坦な接合面で2つに分割可能な内部車室部と、この内部車室部を収容可能な外部車室部と、を有するタービン装置の、少なくとも前記接合面を補修するためのタービン装置補修方法において、前記内部車室部の前記接合面それぞれに形成されて、健全な状態の健全接合面よりも前記各内部車室部が互いに離れる方向に変形して窪むように形成された異常部位を検出して、当該異常部位の変形量を計測する検査工程と、前記検査工程の後に、前記異常部位の表面を所定の面粗さにする下地処理工程と、前記下地処理工程の後に、前記異常部位の少なくとも一部に、少なくともクロム系合金材料を含む溶射材を、前記健全接合面よりも突出する突出部が形成されるように溶射する溶射工程と、前記溶射工程の後に、溶射部の表面位置が、前記健全接合面と同じ位置になるように前記突出部を除去する仕上げ工程と、を有することを特徴とする。   In order to achieve the above object, a turbine apparatus repair method according to the present invention includes a rotor that rotates around an axis, a nozzle that is disposed radially outside the rotor, and a nozzle that can be fixed while covering the nozzle from the radially outer side. In order to repair at least the joint surface of a turbine apparatus having an internal casing part that can be divided into two by a flat joint surface parallel to the shaft and an external casing part that can accommodate the internal compartment part In the turbine apparatus repair method, the inner casing portions are formed on the joint surfaces of the inner casing portions, and the inner casing portions are deformed and recessed in a direction away from each other than the healthy joining surfaces in a healthy state. After detecting the abnormal part and measuring the deformation amount of the abnormal part, after the inspection process, after the base processing process to make the surface of the abnormal part a predetermined surface roughness, after the base processing process ,in front A thermal spraying step of spraying a thermal spray material containing at least a chromium-based alloy material on at least a part of the abnormal part so that a protruding portion protruding from the sound joint surface is formed, and after the thermal spraying step, And a finishing step of removing the protrusion so that the surface position is the same as the sound joint surface.

また、本発明に係るタービン装置補修方法は、軸周りを回転するロータと、このロータの半径方向外側に配置されたノズルと、このノズルを半径方向外側から覆いながら固定可能で軸に平行な平坦な接合面で2つに分割可能な内部車室部と、この内部車室部を収容可能な外部車室部と、を有するタービン装置の、少なくとも前記接合面を補修するためのタービン装置補修方法において、前記内部車室部の前記接合面それぞれに形成されて、健全な状態の健全接合面よりも前記各内部車室部が互いに離れる方向に変形して窪むように形成された異常部位を検出して、当該異常部位の変形量を計測する検査工程と、前記検査工程の後に、一方の前記内部車室部の前記異常部位の表面を所定の面粗さにする下地処理工程と、前記下地処理工程の後に、前記異常部位の少なくとも一部に、少なくともクロム系材料を含む溶射材を、前記健全接合面よりも突出する突出部が形成されるように溶射する溶射工程と、前記突出部の窪み方向突出量が、もう一方の前記内部車室部の前記接合面に形成された前記異常部位の深さとほぼ同じになるように、前記溶射部の表面を除去する仕上げ工程と、を有することを特徴とする。   The turbine device repairing method according to the present invention includes a rotor that rotates around an axis, a nozzle that is disposed radially outside the rotor, and a flat, parallel to the axis that can be fixed while covering the nozzle from the radially outer side. Turbine device repairing method for repairing at least the joint surface of a turbine device having an internal compartment part that can be divided into two at a simple joint surface and an external compartment part that can accommodate the internal compartment part And detecting an abnormal region formed on each of the joint surfaces of the internal casing portion so that the inner casing portions are deformed and recessed in a direction away from the healthy joint surface in a healthy state. An inspection step for measuring a deformation amount of the abnormal portion, a ground treatment step for making the surface of the abnormal portion of one of the internal compartments a predetermined surface roughness after the inspection step, and the ground treatment After the process A thermal spraying process in which a thermal spray material containing at least a chromium-based material is sprayed on at least a part of the abnormal part so that a projecting part projecting from the sound joint surface is formed, and a projecting amount of the projecting part in a recess direction is And a finishing step of removing the surface of the sprayed portion so as to be substantially the same as the depth of the abnormal portion formed on the joint surface of the other internal casing portion.

本発明によれば、タービン装置を効率よく補修することが可能である。   According to the present invention, it is possible to efficiently repair a turbine device.

本発明に係るタービン装置補修方法の第1の実施形態の手順を示すフローチャートである。It is a flowchart which shows the procedure of 1st Embodiment of the turbine apparatus repair method which concerns on this invention. 図1の実施形態の下半外部車室部および下半内部車室部の概略斜視図である。It is a schematic perspective view of the lower half external compartment part and lower half internal compartment part of embodiment of FIG. 図2の下半内部車室部のIII-III矢視概略正断面図で、異常部位を含む接合面の上方に基準バーを配置した状態を示す。FIG. 3 is a schematic cross-sectional view taken along the line III-III in the lower half internal compartment of FIG. 2, showing a state where a reference bar is arranged above the joint surface including the abnormal part. 図3の下半内部車室部の異常部位に下地処理した状態を示す概略部分正断面図である。It is a general | schematic fragmentary front sectional view which shows the state which carried out the base treatment to the abnormal site | part of the lower half internal compartment part of FIG. 図4の異常部位に溶射している状態を示す概略正断面図である。FIG. 5 is a schematic front sectional view showing a state where thermal spraying is performed on the abnormal part of FIG. 4. 図5の溶射が完了した状態を示す概略正断面図である。FIG. 6 is a schematic front sectional view showing a state in which the thermal spraying of FIG. 5 is completed. 図6の余盛層を除去した状態を示す概略正断面図である。It is a general | schematic front sectional view which shows the state which removed the surplus layer of FIG. 本発明に係るタービン装置補修方法の第2の実施形態で、下半内部車室部の接合面の異常部位に溶射材を溶射した状態を示す内部車室部の部分正断面図である。FIG. 6 is a partial front sectional view of an inner casing portion showing a state in which a thermal spray material is sprayed on an abnormal portion of a joint surface of a lower half inner casing portion in the second embodiment of the turbine device repair method according to the present invention. 本発明に係るタービン装置補修方法の第3の実施形態で、下半内部車室部の接合面の異常部位に溶射材を溶射した状態を示す内部車室部の部分正面図である。FIG. 10 is a partial front view of the internal compartment portion showing a state in which a thermal spray material is sprayed on an abnormal portion of the joint surface of the lower half internal compartment portion in the third embodiment of the turbine device repair method according to the present invention. 図9のX-X矢視側面図である。FIG. 10 is a side view taken along the line XX in FIG. 9. 本発明に係るタービン装置補修方法の第4の実施形態で、内部車室部の異常部位付近の部分正面図である。In 4th Embodiment of the turbine apparatus repair method which concerns on this invention, it is a partial front view of the abnormal site | part vicinity of an internal compartment part. 本発明に係るタービン装置補修方法の第5の実施形態で、内部車室部の異常部位を含む断面を示す概略正断面図である。In 5th Embodiment of the turbine apparatus repair method which concerns on this invention, it is a general | schematic front sectional view which shows the cross section containing the abnormal site | part of an internal compartment. 図12の下半内部車室の異常部位に溶射した状態を示す概略正断面図である。FIG. 13 is a schematic front sectional view showing a state where the thermal spraying is performed on the abnormal portion of the lower half internal compartment of FIG. 12.

以下、本発明に係るタービン装置の補修方法の実施形態について、図面を参照して説明する。   Hereinafter, an embodiment of a repair method for a turbine apparatus according to the present invention will be described with reference to the drawings.

[第1の実施形態]
本発明に係るタービン装置の補修方法の第1の実施形態について、図1〜図7を用いて説明する。図1は、本実施形態のタービン装置補修方法の手順を示すフローチャートである。図2は、図1の下半外部車室部1および下半内部車室部2の概略斜視図である。図3は、図2の下半内部車室部2のIII-III矢視概略正断面図で、異常部位20を含む接合面の上方に基準バー10を配置した状態を示す。図4は、図3の下半内部車室部2の異常部位20に下地処理した状態を示す概略部分正断面図である。図5は、図4の異常部位20に溶射している状態を示す概略正断面図である。図6は、図5の溶射が完了した状態を示す概略正断面図である。図7は、図6の余盛層32を除去した状態を示す概略正断面図である。
[First Embodiment]
1st Embodiment of the repair method of the turbine apparatus which concerns on this invention is described using FIGS. FIG. 1 is a flowchart showing the procedure of the turbine apparatus repair method according to the present embodiment. FIG. 2 is a schematic perspective view of the lower half outer casing 1 and the lower half inner casing 2 of FIG. FIG. 3 is a schematic front sectional view taken along the line III-III of the lower half internal compartment 2 of FIG. FIG. 4 is a schematic partial front sectional view showing a state in which the abnormal portion 20 in the lower half inner compartment 2 of FIG. FIG. 5 is a schematic front sectional view showing a state where thermal spraying is performed on the abnormal part 20 of FIG. FIG. 6 is a schematic front sectional view showing a state in which the thermal spraying of FIG. 5 is completed. FIG. 7 is a schematic front sectional view showing a state in which the extra layer 32 of FIG. 6 is removed.

先ず、本実施形態のタービン装置の構成について説明する。   First, the structure of the turbine apparatus of this embodiment is demonstrated.

このタービン装置は水平に延びて水平軸周りを回転するロータ(図示せず)と、このロータの半径方向外側に配置されたノズル(図示せず)と、ノズルを半径方向外側から覆いながら固定する内部車室部2、3と、この内部車室部を収容する外部車室部と、を有する。   The turbine device extends horizontally and rotates around a horizontal axis (not shown), a nozzle (not shown) arranged radially outside the rotor, and fixes the nozzle while covering the nozzle from the outside in the radial direction. It has the internal compartment parts 2 and 3, and the external compartment part which accommodates this internal compartment part.

内部車室2、3は、水平軸を含む水平な分割面(接合面)12、20を境界にして、上下に2つ、すなわち、上半内部車室部3および下半内部車室部2に分割可能である。これら上半内部車室部3および下半内部車室部2は、低炭素鋼で形成されている。   There are two internal casings 2 and 3 on the upper and lower sides of the horizontal dividing surfaces (joint surfaces) 12 and 20 including the horizontal axis, that is, the upper half inner casing 3 and the lower half inner casing 2. Can be divided. The upper half inner casing 3 and the lower half inner casing 2 are made of low carbon steel.

外部車室は、水平軸を含む水平な外部車室分割面1aを境界にして、上半外部車室部(図示せず)および下半外部車室部1に分割可能である。図2では、下半内部車室部2および下半外部車室部1のみを示し、上半側の図示は省略している。   The outer casing can be divided into an upper half outer casing (not shown) and a lower half outer casing 1 with a horizontal outer casing dividing surface 1a including a horizontal axis as a boundary. In FIG. 2, only the lower half internal compartment 2 and the lower half external compartment 1 are shown, and the upper half is not shown.

このように構成のタービン装置を長期間使用すると、上半内部車室部3および下半内部車室部2それぞれの接合面の一部に異常部位20が生じる。ここで、異常部位20が生じていない接合面を健全接合面12とする。異常部位20は、各接合面が互いに離れる方向に変形して、窪むように形成される。この異常部位20は、後で説明するタービン装置補修方法によって、補修される。   When the turbine apparatus configured as described above is used for a long period of time, an abnormal region 20 is generated at a part of the joint surface of each of the upper half internal compartment portion 3 and the lower half internal compartment portion 2. Here, the joint surface where the abnormal part 20 does not occur is referred to as a sound joint surface 12. The abnormal part 20 is formed such that each joint surface is deformed in a direction away from each other and is recessed. The abnormal portion 20 is repaired by a turbine device repair method described later.

以下に、本実施形態のタービン装置補修方法によって、下半内部車室部2の接合面の補修する手順について説明する。   Below, the procedure which repairs the joint surface of the lower half internal compartment part 2 with the turbine apparatus repair method of this embodiment is demonstrated.

タービン装置は、通常、定期的にメンテナンスが行われる。このときに、下半内部車室部2の接合面と、上半内部車室部3の接合面との間に隙間が形成されているか否かを、例えば目視等で検査する。   The turbine apparatus is usually regularly maintained. At this time, whether or not a gap is formed between the joint surface of the lower half internal compartment portion 2 and the joint surface of the upper half internal compartment portion 3 is inspected, for example, visually.

接合面同士の間に隙間が認められたときには、隙間ゲージ等を用いて当該隙間の鉛直方向幅を測定する。上半内部車室部3および下半内部車室部2それぞれの接合面の間に形成される隙間は、各接合面が互いに離れる方向に変形する異常部位20である。ここで、所定値以上の隙間が形成されているとき、すなわち異常部位20が所定値より大きいときには、後述する補修作業を行う。   When a gap is recognized between the joint surfaces, the vertical width of the gap is measured using a gap gauge or the like. A gap formed between the joint surfaces of the upper half internal casing portion 3 and the lower half inner compartment portion 2 is an abnormal portion 20 in which the joint surfaces are deformed in directions away from each other. Here, when a gap of a predetermined value or more is formed, that is, when the abnormal part 20 is larger than the predetermined value, repair work described later is performed.

以下に、下半内部車室部2の接合面の補修作業の手順について図1のフローチャートに基づいて説明する。当該補修作業は、異常部位20に後述する溶射材52を溶射して、使用前の健全な状態にする作業である。   Below, the procedure of the repair operation | work of the joint surface of the lower half internal compartment part 2 is demonstrated based on the flowchart of FIG. The repair work is a work for spraying a thermal spray material 52, which will be described later, on the abnormal part 20 to obtain a healthy state before use.

先ず、図3に示すように、基準バー10を下半内部車室部2の接合面の上方に、回転軸方向に垂直で且つ水平に配置する。基準バー10の詳細な図示は省略しているが、この基準バー10は、鋼材の棒で、配置したときの横断面形状は、アルファベットの「H」を横にしたような形状で、上面および下面それぞれに基準となる水平な測定基準面10aが形成されている。   First, as shown in FIG. 3, the reference bar 10 is disposed above the joint surface of the lower half internal compartment 2 and perpendicular to the rotation axis direction and horizontally. Although the detailed illustration of the reference bar 10 is omitted, the reference bar 10 is a steel bar, and the cross-sectional shape of the reference bar 10 when it is arranged is such that the letter “H” is placed sideways. A horizontal measurement reference surface 10a serving as a reference is formed on each of the lower surfaces.

このとき、接合面のうちロータの回転中心から水平方向両側それぞれに離れた健全な部分、すなわち健全接合面12の上に架台11を設置して、この架台11上面に測定基準面10aが接するように基準バー10を設置する。   At this time, the gantry 11 is installed on a healthy part of the joint surface that is separated from the rotation center of the rotor on both sides in the horizontal direction, that is, the healthy joint surface 12, and the measurement reference surface 10 a is in contact with the upper surface of the gantry 11. The reference bar 10 is installed in

基準バー10を設置した後に、当該測定基準面10aと、異常部位20との鉛直方向距離を測定して、異常部位20の鉛直方向深さを計測する(ステップS1)。具体的には、先ず、測定基準面10aと、健全接合面12との距離を測定して、この距離を基準距離とする。次に、測定基準面10aと、各異状部位との鉛直方向距離を測定して、基準距離との相対的な距離を求めて異常部位20の深さを計測する。   After installing the reference bar 10, the vertical distance between the measurement reference surface 10a and the abnormal part 20 is measured, and the vertical depth of the abnormal part 20 is measured (step S1). Specifically, first, the distance between the measurement reference surface 10a and the sound joint surface 12 is measured, and this distance is set as the reference distance. Next, the vertical distance between the measurement reference surface 10a and each abnormal part is measured, the relative distance from the reference distance is obtained, and the depth of the abnormal part 20 is measured.

次に、異常部位20に形成されたボルト穴(図示せず)等を塞ぐマスキングを行う(ステップS2)。このマスキングは、溶射によって当該ボルト穴等が塞がれてしまうことを抑制するために行うものである。このときボルト穴は、ゴム栓等で塞いでおくとよい。また、異常部位20の周囲の健全な部位(表面)には、マスキングテープ等で覆うとよい。   Next, masking for closing a bolt hole (not shown) formed in the abnormal part 20 is performed (step S2). This masking is performed to prevent the bolt holes from being blocked by thermal spraying. At this time, the bolt hole may be closed with a rubber plug or the like. Further, a healthy part (surface) around the abnormal part 20 may be covered with a masking tape or the like.

次に、図4に示すように、異常部位20の下地処理を行う(ステップS3)。この下地処理では、異常部位20に溶射するときに、溶射材52の密着性を高めるために、異常部位20の表面を所定の面粗さになるようにする。上記の通り、下半内部車室部2は、低炭素鋼で形成されている。炭素鋼の表面を粗くするには、アルミナ等を溶射するプライマー(下塗り)処理を行えばよい。図4の例では、異常部位20の表面上にプライマー処理された下地層25が形成されている。   Next, as shown in FIG. 4, the background processing of the abnormal part 20 is performed (step S3). In this base treatment, when the thermal spraying is performed on the abnormal part 20, the surface of the abnormal part 20 is made to have a predetermined surface roughness in order to improve the adhesion of the sprayed material 52. As described above, the lower half internal casing 2 is made of low carbon steel. In order to roughen the surface of the carbon steel, a primer (undercoat) treatment for spraying alumina or the like may be performed. In the example of FIG. 4, the primer layer 25 is formed on the surface of the abnormal part 20.

この下地処理は、所定の面粗さになればよく、アルミナ溶射等に限らない。下地層25を形成することなく、例えばグライダ等で機械的に面粗さを粗くしてもよい。   The ground treatment is not limited to alumina spraying or the like as long as the surface roughness is a predetermined surface roughness. The surface roughness may be mechanically roughened by, for example, a glider without forming the base layer 25.

下地処理の後に、図5に示すように、異常部位20の溶射材52を吹き付ける溶射を行う(ステップS4)。溶射装置50の構成について詳細な説明は省略するが、ワイヤ状の溶射材52をアセチレンガスや酸素等で燃焼させて溶かした状態で、異常部位20に吹き付けるように構成されている。   After the ground treatment, as shown in FIG. 5, thermal spraying is performed by spraying the thermal spray material 52 on the abnormal part 20 (step S4). Although a detailed description of the configuration of the thermal spraying device 50 is omitted, the thermal spraying device 52 is configured to be sprayed onto the abnormal site 20 in a state where the wire-shaped thermal spray material 52 is burned and melted with acetylene gas or oxygen.

このとき、溶射材52が溶射されて形成される溶射層30は、図6に示すように、健全接合面12よりも上方に突出する突出部(余盛層)32が形成されるまで溶射する。溶射層30は、余盛層32と、異常部位20に埋め盛られた有効溶射層31を含む。ここで、溶射材52は、下半内部車室部2の材質(低炭素鋼)と同系の合金材料がよい。また、本実施形態では、溶射材52にクロム系合金材料を含有させている。これにより、密着性、耐衝撃性、耐食性等を高めることができる。   At this time, the thermal spray layer 30 formed by thermal spraying of the thermal spray material 52 is sprayed until a protruding portion (excess layer) 32 protruding upward from the sound joint surface 12 is formed as shown in FIG. . The thermal spray layer 30 includes a surplus layer 32 and an effective thermal spray layer 31 buried in the abnormal part 20. Here, the thermal spray material 52 is preferably an alloy material similar to the material (low carbon steel) of the lower half inner casing 2. In the present embodiment, the thermal spray material 52 contains a chromium-based alloy material. Thereby, adhesiveness, impact resistance, corrosion resistance, etc. can be improved.

また、溶射の方法は、メタルスプレー法、アーク法等の一般的な溶射方法を用いることができる。   Further, as a spraying method, a general spraying method such as a metal spray method or an arc method can be used.

次に、図7に示すように、溶射層30の上面が健全接合面12と同じ位置になるように、すなわち、溶射層30の表面と健全接合面12が同じ平面上にあるように、除去装置等によって余盛層32を除去する(ステップS5)。これにより、有効溶射層31が残った状態になる。   Next, as shown in FIG. 7, the thermal spray layer 30 is removed so that the upper surface of the thermal spray layer 30 is at the same position as the sound bonding surface 12, that is, the surface of the thermal spray layer 30 and the healthy bonding surface 12 are on the same plane. The extra layer 32 is removed by an apparatus or the like (step S5). As a result, the effective sprayed layer 31 remains.

この除去装置の詳細な図示は省略しているが、水平移動可能距離が1m程度の簡易フライス加工機等を下半内部車室部2の上方に配置して、当該装置に正面フライス41等の工具を取り付けて切削加工する。これにより、余盛層32を除去すると共に、有効溶射層31の表面が平坦になるように仕上げることができる。   Although a detailed illustration of this removal device is omitted, a simple milling machine or the like having a horizontal movable distance of about 1 m is disposed above the lower half internal compartment 2 and the front milling device 41 or the like is placed in the device. Cutting with a tool attached. Thereby, while removing the surplus layer 32, it can finish so that the surface of the effective sprayed layer 31 may become flat.

この後に、有効溶射層31の表面に形成されたツールマーク等をグラインダ等で除去して、有効溶射層31の表面が健全接合面12と同等の表面粗さになるように仕上げる(ステップS6)。この後に有効溶射層31が剥離していないこと等を検査する(ステップS7)。この検査で、有効溶射層31の表面が、健全接合面12と同じ位置になっているか否かを、基準バー10等を用いて再度検査してもよい。また、基準バー10の測定基準面10aを、有効溶射層31の表面に接触させて、平坦度を目視検査してもよい。以上の手順によって、補修作業が完了する。   Thereafter, tool marks and the like formed on the surface of the effective sprayed layer 31 are removed by a grinder or the like, and the surface of the effective sprayed layer 31 is finished to have a surface roughness equivalent to that of the sound joint surface 12 (step S6). . Thereafter, it is inspected that the effective sprayed layer 31 is not peeled off (step S7). In this inspection, whether or not the surface of the effective sprayed layer 31 is in the same position as the sound joint surface 12 may be inspected again using the reference bar 10 or the like. Further, the measurement reference surface 10a of the reference bar 10 may be brought into contact with the surface of the effective sprayed layer 31, and the flatness may be visually inspected. The repair work is completed by the above procedure.

以上の説明からわかるように本実施形態によれば、予め異常部位20の鉛直方向距離(深さ)を計測しているため、溶射材52を溶射する量等を最適に調整して、溶射層30の厚みを所定値にすることが可能なる。また、溶射材52にクロム系合金材料を含有させているため、密着性等が向上するため、高品質な溶射層30を得ることができる。   As can be seen from the above description, according to the present embodiment, since the vertical distance (depth) of the abnormal region 20 is measured in advance, the amount of the thermal spraying material 52 to be sprayed is optimally adjusted, and the sprayed layer. The thickness of 30 can be set to a predetermined value. In addition, since the thermal spray material 52 contains a chromium-based alloy material, adhesion and the like are improved, so that a high-quality thermal spray layer 30 can be obtained.

また、当該補修方法は、異常部位20を溶射するだけで、異常部位20以外の健全な部位はほとんど加工しない。このため、補修時に健全な部位も含めて内部車室部2、3の形状を再び加工する必要がない。よって、当該異常部位20を効率よく使用前の正常な状態に補修することが可能である。   Moreover, the said repair method only sprays the abnormal site | part 20, and does not process the healthy site | parts other than the abnormal site | part 20 almost. For this reason, it is not necessary to process the shape of the internal compartment parts 2 and 3 again including a healthy part at the time of repair. Therefore, the abnormal part 20 can be efficiently repaired to a normal state before use.

また、当該補修方法は、タービン装置が設置されている現場で、内部車室部2、3の補修を行うことができるため、内部車室部2、3等を移送するための時間が不要になり、補修工期を短縮することができる。   Moreover, since the said repair method can repair the internal compartment parts 2 and 3 at the site | part in which the turbine apparatus is installed, the time for transferring the internal compartment parts 2 and 3 etc. is unnecessary. Thus, the repair period can be shortened.

[第2の実施形態]
本発明に係るタービン装置の補修方法の第2の実施形態について、図1および図8を用いて説明する。図8は、本実施形態のタービン装置補修方法で下半内部車室部2の接合面の異常部位20に溶射材52を溶射した状態を示す下半内部車室部2の部分正断面図である。なお、本実施形態は、第1の実施形態の変形例であって、第1の実施形態と同一部分または類似部分には、同一符号を付して、重複説明を省略する。
[Second Embodiment]
A second embodiment of the turbine apparatus repair method according to the present invention will be described with reference to FIGS. 1 and 8. FIG. 8 is a partial front sectional view of the lower half inner casing 2 showing a state in which the sprayed material 52 is sprayed on the abnormal portion 20 on the joint surface of the lower half inner casing 2 by the turbine device repair method of the present embodiment. is there. In addition, this embodiment is a modification of 1st Embodiment, Comprising: The same code | symbol is attached | subjected to the same part or similar part as 1st Embodiment, and duplication description is abbreviate | omitted.

第1の実施形態では、異常部位20の深さが浅い場合(例えば1mm以下)には、余盛層32を除去するときに、有効溶射層31の厚みが極端に薄くなる場合がある。この場合、余盛層32を除去しているときに、有効溶射層31が剥離してしまう可能性がある。   In the first embodiment, when the depth of the abnormal portion 20 is shallow (for example, 1 mm or less), the thickness of the effective sprayed layer 31 may be extremely thin when the surplus layer 32 is removed. In this case, when the surplus layer 32 is removed, the effective sprayed layer 31 may be peeled off.

本実施形態は、検査工程(ステップS1)の後で下地処理工程(ステップS2)の前に、異常部位20を、窪んでいる方向に所定の量だけ掘り下げて、除去部27を形成する除去工程を有する。有効溶射層31の厚みが約1mmになるように、当該異常部位20を掘り下げるとよい。   In the present embodiment, after the inspection process (step S1) and before the ground treatment process (step S2), the removal portion 27 is formed by digging the abnormal part 20 by a predetermined amount in the recessed direction. Have The abnormal portion 20 may be dug down so that the effective sprayed layer 31 has a thickness of about 1 mm.

これにより、有効溶射層31の剥離等の不具合を抑制することが可能になり、第1の実施形態に比べて、補修の仕上がり品質が向上する。   Thereby, it becomes possible to suppress defects, such as peeling of the effective sprayed layer 31, and the finishing quality of repair improves compared with 1st Embodiment.

[第3の実施形態]
本発明に係るタービン装置の補修方法の第3の実施形態について、図9および図10を用いて説明する。図9は、本実施形態のタービン装置補修方法で、下半内部車室部2の接合面の異常部位20に溶射材52を溶射した状態を示す下半内部車室部2の部分正面図である。図10は、図9のX-X矢視側面図である。なお、本実施形態は、第1の実施形態の変形例であって、第1の実施形態と同一部分または類似部分には、同一符号を付して、重複説明を省略する。
[Third Embodiment]
A third embodiment of the turbine apparatus repair method according to the present invention will be described with reference to FIGS. 9 and 10. FIG. 9 is a partial front view of the lower half internal compartment portion 2 showing a state in which the thermal spray material 52 is sprayed on the abnormal portion 20 on the joint surface of the lower half internal compartment portion 2 in the turbine device repair method of the present embodiment. is there. FIG. 10 is a side view taken along arrow XX in FIG. In addition, this embodiment is a modification of 1st Embodiment, Comprising: The same code | symbol is attached | subjected to the same part or similar part as 1st Embodiment, and duplication description is abbreviate | omitted.

通常、健全接合面12は、ロータの回転軸から離れた部位、すなわち水平方向外側にあることが多く、異常部位20は、当該回転軸に近い側、すなわち内側であることが多い。このため、第1の実施形態では、異常部位20に溶射をするときに、溶射層30の厚みを確認しにくいことがある。   Usually, the sound joint surface 12 is often located at a position away from the rotation axis of the rotor, that is, outside in the horizontal direction, and the abnormal area 20 is often located near the rotation axis, that is, inside. For this reason, in the first embodiment, it may be difficult to confirm the thickness of the sprayed layer 30 when spraying the abnormal site 20.

本実施形態では、下地処理工程(ステップS3)の後で溶射工程(ステップS4)の前に、異常部位20の底部から健全接合面12までの距離を把握するための基準部材61を設置する基準部材設置工程を有する。   In this embodiment, the reference | standard which installs the reference | standard member 61 for grasping | ascertaining the distance from the bottom part of the abnormal site | part 20 to the healthy joining surface 12 before a thermal spraying process (step S4) after a base treatment process (step S3). It has a member installation process.

この基準部材61は、直方体の形状で、異常部位20付近に配置される。このとき、当該基準部材61の上面および下面が、水平になるように配置される。ここで、配置された基準部材61の下面と、健全接合面12との鉛直距離を予め計測する。これにより、溶射するときに、当該下面と、溶射層30の表面とを鉛直方向距離(図中のh)を測定することで、溶射層30の厚みを所定値になるようにすることができる。すなわち、溶射工程(ステップS4)は、基準部材61の下面から溶射層30の表面までの距離hを測定する工程が含まれる。   The reference member 61 has a rectangular parallelepiped shape and is disposed near the abnormal site 20. At this time, the upper and lower surfaces of the reference member 61 are arranged to be horizontal. Here, the vertical distance between the lower surface of the arranged reference member 61 and the sound joint surface 12 is measured in advance. Thereby, when spraying, the thickness of the sprayed layer 30 can be set to a predetermined value by measuring the vertical distance (h in the figure) between the lower surface and the surface of the sprayed layer 30. . That is, the thermal spraying step (step S4) includes a step of measuring the distance h from the lower surface of the reference member 61 to the surface of the thermal spray layer 30.

これにより、余分な溶射層30が形成されることが抑制されるため、第1の実施形態に比べて、溶射のための作業時間を少なくすることが可能となり、工期を短縮できる。   Thereby, since it is suppressed that the excessive spraying layer 30 is formed, it becomes possible to reduce the working time for thermal spraying compared with 1st Embodiment, and can shorten a construction period.

[第4の実施形態]
本発明に係るタービン装置の補修方法の第4の実施形態について、図11を用いて説明する。図11は、本実施形態のタービン装置補修方法で、下半内部車室部2の異常部位20付近の部分正面図である。なお、本実施形態は、第1の実施形態の変形例であって、第1の実施形態と同一部分または類似部分には、同一符号を付して、重複説明を省略する。
[Fourth Embodiment]
A fourth embodiment of the turbine apparatus repair method according to the present invention will be described with reference to FIG. FIG. 11 is a partial front view of the vicinity of the abnormal part 20 in the lower half internal compartment 2 in the turbine device repair method according to the present embodiment. In addition, this embodiment is a modification of 1st Embodiment, Comprising: The same code | symbol is attached | subjected to the same part or similar part as 1st Embodiment, and duplication description is abbreviate | omitted.

本実施形態は、溶射工程(ステップS4)の後で余盛層32を除去する(ステップS5)前に、溶射層30の表面を加熱装置71で350℃程度に加熱する加熱工程を有する。これにより、余盛層32の除去加工等を容易に行うことができ、補修作業時間を短縮することができる。よって、第1の実施形態に比べて工期を短縮することができる。   The present embodiment includes a heating process in which the surface of the thermal spray layer 30 is heated to about 350 ° C. by the heating device 71 before the surfacing layer 32 is removed (step S5) after the thermal spray process (step S4). Thereby, the removal process etc. of the surplus layer 32 can be performed easily, and repair work time can be shortened. Therefore, the construction period can be shortened compared to the first embodiment.

[第5の実施形態]
本発明に係るタービン装置の補修方法の第5の実施形態について、図12および図13を用いて説明する。図12は、本実施形態のタービン装置補修方法で、内部車室部の異常部位20を含む断面を示す概略正断面図である。図13は、図12の下半内部車室の異常部位20に溶射材52を溶射した状態を示す概略正断面図である。なお、本実施形態は、第1の実施形態の変形例であって、第1の実施形態と同一部分または類似部分には、同一符号を付して、重複説明を省略する。
[Fifth Embodiment]
A fifth embodiment of the turbine apparatus repair method according to the present invention will be described with reference to FIGS. 12 and 13. FIG. 12 is a schematic front sectional view showing a cross section including the abnormal portion 20 of the internal compartment in the turbine device repair method of the present embodiment. FIG. 13 is a schematic front sectional view showing a state in which the thermal spray material 52 is sprayed on the abnormal part 20 in the lower half internal compartment of FIG. In addition, this embodiment is a modification of 1st Embodiment, Comprising: The same code | symbol is attached | subjected to the same part or similar part as 1st Embodiment, and duplication description is abbreviate | omitted.

本実施形態の補修方法は、下半内部車室部2の接合面の異常部位20を計測すると共に、上半内部車室部3の接合面の異常部位20も計測する。図12に示すように、上半内部車室部3および下半内部車室部2それぞれの接合面は、ほぼ同じように変形することが多い。   The repair method of the present embodiment measures the abnormal part 20 on the joint surface of the lower half internal compartment 2 and also measures the abnormal part 20 on the joint surface of the upper half internal compartment 3. As shown in FIG. 12, the joint surfaces of the upper half internal compartment 3 and the lower half internal compartment 2 are often deformed in substantially the same manner.

第1〜第4の実施形態は、下半内部車室部2の接合面を、使用前の状態、すなわち平坦な水平面になるように仕上げている。これに対して、本実施形態では、図13に示すように、下半内部車室部2の接合面の異常部位20に溶射するときに、健全接合面12よりも上方に突出させる。このときの突出量は、上半内部車室部3の接合面の異常部位20の窪み分と同じになるように調整する。   In the first to fourth embodiments, the joint surface of the lower half inner compartment 2 is finished so as to be in a state before use, that is, a flat horizontal surface. On the other hand, in this embodiment, as shown in FIG. 13, when spraying to the abnormal part 20 of the joint surface of the lower half internal vehicle compartment 2, it protrudes above the sound joint surface 12. The amount of protrusion at this time is adjusted so as to be the same as the amount of depression of the abnormal portion 20 on the joint surface of the upper half internal casing 3.

これにより、上半内部車室部3の接合面を溶射する工程を省けるため、より短時間で補修作業を行うことが可能になる。   As a result, since the step of spraying the joint surface of the upper half internal compartment 3 can be omitted, the repair work can be performed in a shorter time.

[その他の実施形態]
上記実施形態の説明は、本発明を説明するための例示であって、特許請求の範囲に記載の発明を限定するものではない。また、本発明の各部構成は上記実施形態に限らず、特許請求の範囲に記載の技術的範囲内で種々の変形が可能である。
[Other Embodiments]
The description of the above embodiment is an example for explaining the present invention, and does not limit the invention described in the claims. Moreover, each part structure of this invention is not restricted to the said embodiment, A various deformation | transformation is possible within the technical scope as described in a claim.

例えば、第1〜第4の実施形態の特徴を互いに組み合わせることが可能である。また、第5の実施形態の特徴に、第2〜第4の実施形態の特徴を組み合わせることも可能である。   For example, the features of the first to fourth embodiments can be combined with each other. Moreover, it is also possible to combine the features of the second to fourth embodiments with the features of the fifth embodiment.

1…下半外部車室部、1a…外部車室分割面、2…下半内部車室部、3…上半内部車室部、10…基準バー、10a…測定基準面、11…架台、12…健全接合面、20…異常部位、25…下地層、27…除去部、30…溶射層、31…有効溶射層、32…突出部(余盛層)、41…正面フライス、50…溶射装置、52…溶射材、61…基準部材、71…加熱装置 DESCRIPTION OF SYMBOLS 1 ... Lower half external compartment part, 1a ... External compartment division surface, 2 ... Lower half internal compartment part, 3 ... Upper half internal compartment part, 10 ... Reference | standard bar, 10a ... Measurement reference plane, 11 ... Mounting stand, DESCRIPTION OF SYMBOLS 12 ... Sound joint surface, 20 ... Abnormal site | part, 25 ... Underlayer, 27 ... Removal part, 30 ... Sprayed layer, 31 ... Effective sprayed layer, 32 ... Protruding part (excess layer), 41 ... Front milling, 50 ... Spraying Device 52 ... Thermal spray material 61 ... Reference member 71 ... Heating device

Claims (6)

軸周りを回転するロータと、このロータの半径方向外側に配置されたノズルと、このノズルを半径方向外側から覆いながら固定可能で軸に平行な平坦な接合面で2つに分割可能な内部車室部と、この内部車室部を収容可能な外部車室部と、を有するタービン装置の、少なくとも前記接合面を補修するためのタービン装置補修方法において、
前記内部車室部の前記接合面それぞれに形成されて、健全な状態の健全接合面よりも前記各内部車室部が互いに離れる方向に変形して窪むように形成された異常部位を検出して、当該異常部位の変形量を計測する検査工程と、
前記検査工程の後に、前記異常部位の表面を所定の面粗さにする下地処理工程と、
前記下地処理工程の後に、前記異常部位の少なくとも一部に、少なくともクロム系合金材料を含む溶射材を、前記健全接合面よりも突出する突出部が形成されるように溶射する溶射工程と、
前記溶射工程の後に、溶射部の表面位置が、前記健全接合面と同じ位置になるように前記突出部を除去する仕上げ工程と、
を有することを特徴とするタービン装置補修方法。
A rotor that rotates around an axis, a nozzle arranged radially outside the rotor, and an internal vehicle that can be divided into two at a flat joint surface parallel to the axis that can be fixed while covering the nozzle from the outside in the radial direction In a turbine apparatus repairing method for repairing at least the joint surface of a turbine apparatus having a chamber section and an external casing section capable of accommodating the internal casing section,
Detected abnormal portions formed on each of the joint surfaces of the internal casing portion, the inner casing portions being deformed and recessed in a direction away from each other than a healthy joint surface in a healthy state, An inspection process for measuring the deformation amount of the abnormal part;
After the inspection step, a surface treatment step for making the surface of the abnormal part a predetermined surface roughness,
A thermal spraying step of spraying a thermal spray material containing at least a chromium-based alloy material on at least a part of the abnormal site after the base treatment step so that a protruding portion protruding from the sound joint surface is formed;
After the thermal spraying step, a finishing step of removing the protrusion so that the surface position of the thermal spray portion is the same position as the sound joint surface,
A turbine device repairing method characterized by comprising:
前記下地処理工程は、アルミナ材を含む溶射材を溶射する工程を含むことを特徴とする請求項1に記載のタービン装置補修方法。   The turbine apparatus repair method according to claim 1, wherein the surface treatment step includes a step of spraying a thermal spray material containing an alumina material. 前記検査工程の後で前記下地処理工程の前に、前記異常部位を、窪んでいる方向に所定の量だけ掘り下げるように除去する除去工程を有すること、を特徴とする請求項1または請求項2に記載のタービン装置補修方法。   3. The method according to claim 1, further comprising a removal step of removing the abnormal portion so as to dig a predetermined amount in the direction of depression after the inspection step and before the base treatment step. The turbine apparatus repair method described in 1. 前記溶射工程の後で前記仕上げ工程の前に、前記溶射部の表面を加熱する加熱工程を有することを特徴とする請求項1ないし請求項3のいずれか一項に記載のタービン装置補修方法。   The turbine apparatus repair method according to any one of claims 1 to 3, further comprising a heating step of heating a surface of the sprayed portion after the spraying step and before the finishing step. 前記下地処理工程の後で前記溶射工程の前に、前記異常部位の底部から前記健全接合面までの距離を把握するための基準部材を、前記異常部位のうち前記健全接合面が広がる方向に前記健全接合面から離れた位置に設置する基準部材設置工程と、
前記基準部材設置工程の後で前記溶射工程の前に、前記基準部材の底面から前記健全接合面までの基準距離を測定する基準距離測定工程と、
を有し、
前記溶射工程は、前記基準部材の底面から溶射部の表面までの距離を測定する工程を含むこと、
を特徴とする請求項1ないし請求項4のいずれか一項に記載のタービン装置補修方法。
After the base treatment step and before the thermal spraying step, a reference member for grasping the distance from the bottom of the abnormal part to the healthy joint surface, in the direction in which the healthy joint surface spreads among the abnormal parts, A reference member installation process to be installed at a position away from the sound joint surface;
A reference distance measuring step for measuring a reference distance from a bottom surface of the reference member to the sound joint surface after the reference member installation step and before the spraying step;
Have
The thermal spraying step includes a step of measuring a distance from a bottom surface of the reference member to a surface of the thermal spray portion;
The turbine apparatus repair method according to any one of claims 1 to 4, wherein
軸周りを回転するロータと、このロータの半径方向外側に配置されたノズルと、このノズルを半径方向外側から覆いながら固定可能で軸に平行な平坦な接合面で2つに分割可能な内部車室部と、この内部車室部を収容可能な外部車室部と、を有するタービン装置の、少なくとも前記接合面を補修するためのタービン装置補修方法において、
前記内部車室部の前記接合面それぞれに形成されて、健全な状態の健全接合面よりも前記各内部車室部が互いに離れる方向に変形して窪むように形成された異常部位を検出して、当該異常部位の変形量を計測する検査工程と、
前記検査工程の後に、一方の前記内部車室部の前記異常部位の表面を所定の面粗さにする下地処理工程と、
前記下地処理工程の後に、前記異常部位の少なくとも一部に、少なくともクロム系材料を含む溶射材を、前記健全接合面よりも突出する突出部が形成されるように溶射する溶射工程と、
前記突出部の窪み方向突出量が、もう一方の前記内部車室部の前記接合面に形成された前記異常部位の深さとほぼ同じになるように、前記溶射部の表面を除去する仕上げ工程と、
を有することを特徴とするタービン装置補修方法。
A rotor that rotates around an axis, a nozzle arranged radially outside the rotor, and an internal vehicle that can be divided into two at a flat joint surface parallel to the axis that can be fixed while covering the nozzle from the outside in the radial direction In a turbine apparatus repairing method for repairing at least the joint surface of a turbine apparatus having a chamber section and an external casing section capable of accommodating the internal casing section,
Detected abnormal portions formed on each of the joint surfaces of the internal casing portion, the inner casing portions being deformed and recessed in a direction away from each other than a healthy joint surface in a healthy state, An inspection process for measuring the deformation amount of the abnormal part;
After the inspection step, a surface treatment step of making the surface of the abnormal part of one of the internal compartments a predetermined surface roughness,
After the base treatment step, a thermal spraying step of spraying a thermal spray material containing at least a chromium-based material on at least a part of the abnormal site so that a protruding portion protruding from the sound joint surface is formed;
A finishing step of removing the surface of the sprayed portion so that the protruding amount of the protruding portion in the recess direction is substantially the same as the depth of the abnormal portion formed on the joint surface of the other internal casing portion; ,
A turbine device repairing method characterized by comprising:
JP2009238204A 2009-10-15 2009-10-15 Turbine equipment repair method Expired - Fee Related JP5355343B2 (en)