JP2001314968A - Welding wire charged article - Google Patents

Welding wire charged article

Info

Publication number
JP2001314968A
JP2001314968A JP2000133835A JP2000133835A JP2001314968A JP 2001314968 A JP2001314968 A JP 2001314968A JP 2000133835 A JP2000133835 A JP 2000133835A JP 2000133835 A JP2000133835 A JP 2000133835A JP 2001314968 A JP2001314968 A JP 2001314968A
Authority
JP
Japan
Prior art keywords
inner cylinder
welding wire
wire
welding
loops
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Withdrawn
Application number
JP2000133835A
Other languages
Japanese (ja)
Inventor
Tadamori Kumada
忠盛 熊田
Tadami Adachi
忠美 足立
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Nippon Steel Welding and Engineering Co Ltd
Original Assignee
Nippon Steel Welding and Engineering Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Nippon Steel Welding and Engineering Co Ltd filed Critical Nippon Steel Welding and Engineering Co Ltd
Priority to JP2000133835A priority Critical patent/JP2001314968A/en
Publication of JP2001314968A publication Critical patent/JP2001314968A/en
Withdrawn legal-status Critical Current

Abstract

PROBLEM TO BE SOLVED: To provide a welding wire charged article from which welding wire can be taken out smoothly without coiling around an inner cylinder, even if a plurality of loops are drawn out in taking out welding wire stored built-up in a pail receptacle. SOLUTION: The twisted welding wire charged article stored built up in a loop state between an outer cylinder forming the paid receptacle and an inner cylinder fixed on the bottom of the pail receptacle, is characterized in that an inner cylinder is a cardboard liner having thickness of 0.8-1.5 mm and weight of 400 g/m2 or more, and charged with twisted welding wire.

Description

【発明の詳細な説明】DETAILED DESCRIPTION OF THE INVENTION

【0001】[0001]

【発明の属する技術分野】本発明は、ペイル容器に捩り
入りのソリッドワイヤやフラックス入りワイヤの溶接用
ワイヤをループ状に積層収納した溶接用ワイヤの装填物
に関する。
BACKGROUND OF THE INVENTION 1. Field of the Invention The present invention relates to a welding wire charge in which a welding wire for a twisted solid wire or a flux-cored wire is stacked and housed in a loop shape in a pail container.

【0002】[0002]

【従来の技術】200〜350kgの溶接用ワイヤの収納
容器として一般にペイル容器が使用されるが、収納され
た溶接用ワイヤは、弾性限界の範囲内で捩られ、例えば
250〜360°の捩りを与えられて所定のループ径で
花模様状に積層収納されている。したがって、溶接用ワ
イヤはペイル容器内で捩りを戻そうとする力が働き、ワ
イヤを自由にするとペイル容器の軸方向に跳ねようとす
る性質を有するので、ワイヤ取り出し時にからみやもつ
れが発生する。このため、従来から例えば特公昭59−
8474号公報にあるように、ペイル容器内のワイヤル
ープ上に円環状の押さえ板を載置して、ワイヤを上から
押さえることにより解決する方法が提案されている。
2. Description of the Related Art Generally, a pail container is used as a storage container for a welding wire of 200 to 350 kg. The stored welding wire is twisted within a range of elasticity limit, for example, a twist of 250 to 360 °. It is provided and stored in a flower pattern with a predetermined loop diameter. Therefore, the welding wire has a property of returning the torsion in the pail container, and has a property of bouncing in the axial direction of the pail container when the wire is free. Therefore, entanglement or tangling occurs when the wire is taken out. For this reason, conventionally, for example,
As disclosed in Japanese Patent No. 8474, a method has been proposed in which an annular holding plate is placed on a wire loop in a pail container and the wire is pressed from above.

【0003】図3は、前記特公昭59−8474号公報
記載の、ペイル容器に積層収納された溶接用ワイヤの取
り出し状態を示した断面図で、ペイル容器7を構成する
外筒1の内部に、捩り入りの溶接用ワイヤ5がループ状
に積層収納されている。この溶接用ワイヤ5は、積層体
2の積層によって形成された円柱状の空洞にペイル容器
7の底部8に固設された内筒6を備え、該積層体2と内
筒6の間に円筒状空洞4を形成する。
FIG. 3 is a cross-sectional view showing a state in which welding wires stacked and housed in a pail container are taken out, described in Japanese Patent Publication No. Sho 59-8474, in which the inside of an outer cylinder 1 constituting a pail container 7 is shown. The twisted welding wires 5 are stacked and stored in a loop shape. The welding wire 5 includes an inner cylinder 6 fixed to a bottom portion 8 of a pail container 7 in a cylindrical cavity formed by laminating the laminate 2, and a cylinder between the laminate 2 and the inner cylinder 6. A cavity 4 is formed.

【0004】積層体2の上部には押さえ板3が載置さ
れ、溶接用ワイヤの跳ね上がりを防止している。また前
記内筒6は、溶接用ワイヤ5が円筒状空洞4に複数のル
プが引き出された場合に円柱状空洞4で捩りを解除しよ
うとして跳ね上がるのを防止している。
[0004] A pressing plate 3 is placed on the upper part of the laminate 2 to prevent the welding wire from jumping up. Further, the inner tube 6 prevents the welding wire 5 from jumping up in an attempt to release the torsion in the cylindrical cavity 4 when a plurality of loops are pulled out into the cylindrical cavity 4.

【0005】しかし図4に示すように、円筒状空洞4に
複数のループが引き出されても、円筒6があるので円柱
状空洞4部で跳ね上がることはないが、特に積層体2の
積層高さが低いときに円筒空洞4に引き出された複数ル
ープの溶接用ワイヤ5は、図示しない取り出し装置また
は取り出し案内部材より順次引き上げられるが、ループ
径が小さくなって内筒6に巻き付いて上方への円滑な移
動ができなくなる。したがって、溶接機のワイヤ送給装
置において大きな抵抗となり、ワイヤ送給速度が一定と
ならず溶接アークが不安定となったり、ワイヤ送給がで
きなくなって溶接が停止する場合がある。
However, as shown in FIG. 4, even if a plurality of loops are drawn out to the cylindrical cavity 4, the cylinder 6 does not cause the cylindrical cavity 4 to jump up. The welding wire 5 having a plurality of loops drawn out into the cylindrical cavity 4 when the height is low is sequentially pulled up by a take-out device or a take-out guide member (not shown). Can not move. Therefore, a large resistance is generated in the wire feeding device of the welding machine, and the wire feeding speed may not be constant, and the welding arc may be unstable, or the wire feeding may not be performed, and the welding may be stopped.

【0006】[0006]

【発明が解決しようとする課題】本発明は、ペイル容器
に積層収納された溶接用ワイヤを取り出す際、複数のル
ープが引き出された場合においても、溶接用ワイヤが内
筒に巻き付くことなく、円滑に取り出すことができる溶
接用ワイヤの装填物を提供することを目的とする。
SUMMARY OF THE INVENTION According to the present invention, when a plurality of loops are pulled out when a welding wire stacked and housed in a pail container is taken out, the welding wire does not wrap around the inner cylinder. An object of the present invention is to provide a charge of a welding wire that can be smoothly removed.

【0007】[0007]

【課題を解決するための手段】本発明の要旨は、ペイル
容器を構成する外筒と該ペール容器の底部に固設された
内筒との間にループ状に積層収納した捩り入り溶接用ワ
イヤの装填物において、内筒は、その厚さが0.8〜
1.5mmで、かつ秤量が400g/m2 以上の段ボー
ル用ライナであり、捩り入り溶接用ワイヤを装填したこ
とを特徴とする溶接用ワイヤの装填物にある。
SUMMARY OF THE INVENTION The gist of the present invention is to provide a twisted welding wire laminated and housed between an outer cylinder constituting a pail container and an inner cylinder fixed to the bottom of the pail container. The inner cylinder has a thickness of 0.8 to
It is a liner for corrugated cardboard having a thickness of 1.5 mm and a weighing of 400 g / m 2 or more, and is characterized by being loaded with a torsion welding wire.

【0008】[0008]

【発明の実施の形態】図1は、本発明の溶接用ワイヤの
装填物を用いて溶接用ワイヤを取り出す状態を示す断面
図である。ペイル容器7を構成する外筒1と、ペイル容
器7の底部8に固設された内筒6との間に、捩り入りの
溶接用ワイヤがループ状に積層収納されている。この溶
接用ワイヤ5は、積層体2の積層によって形成された円
柱状の空洞にペイル容器7の底部8に固設された内筒6
を備え、該積層体2と内筒6の間に円筒状空洞4を形成
する。
FIG. 1 is a sectional view showing a state in which a welding wire is taken out by using a charge of the welding wire of the present invention. Between the outer cylinder 1 constituting the pail container 7 and the inner cylinder 6 fixed to the bottom portion 8 of the pail container 7, a welding wire with a twist is stacked and stored in a loop shape. The welding wire 5 is provided with an inner cylinder 6 fixed to a bottom 8 of a pail container 7 in a cylindrical cavity formed by laminating the laminate 2.
And a cylindrical cavity 4 is formed between the laminate 2 and the inner cylinder 6.

【0009】積層体2の上部には押さえ板3が載置さ
れ、溶接用ワイヤの跳ね上がりを防止している。また前
記内筒6は、溶接用ワイヤ5が円筒状空洞4に複数のル
ープが引き出された場合に、円柱状空洞4で捩りを解除
しようとして跳ね上がるのを防止している。
A pressing plate 3 is placed on the upper part of the laminate 2 to prevent the welding wire from jumping up. In addition, the inner tube 6 prevents the welding wire 5 from jumping to release the twist in the cylindrical cavity 4 when a plurality of loops are drawn out into the cylindrical cavity 4.

【0010】本発明においては、内筒6が厚さ0.8〜
1.5mmの段ボール用ライナであり、図1および図1
のA−A′断面を、図2に示すように内筒6の外周長が
先端部になるほど小となるように変形するので、複数の
ループが引き出された場合でも、溶接用ワイヤ5は内筒
6の外面に沿って順序よく上昇して、図示しないワイヤ
取り出し装置または取り出し案内部材に導かれる。した
がって、引き出された複数のループは内筒6に巻き付く
ことなく、その表面を抵抗なく滑って上昇するため、円
滑に引き出すことができる。
In the present invention, the inner cylinder 6 has a thickness of 0.8 to 0.8.
1.5 mm corrugated cardboard liner, FIG. 1 and FIG.
2 is deformed so that the outer peripheral length of the inner cylinder 6 becomes smaller toward the tip end as shown in FIG. 2, so that even when a plurality of loops are pulled out, the welding wire 5 is It rises in order along the outer surface of the cylinder 6 and is guided to a wire take-out device or take-out guide member (not shown). Therefore, the plurality of loops that are pulled out are wrapped around the inner cylinder 6 without any resistance, and slide upward without any resistance, so that the loops can be pulled out smoothly.

【0011】内筒6に使用する段ボール用ライナの厚さ
が0.8mm未満であると、引き出された複数のループ
によって内筒6が部分的に締め付けられて変形し、ルー
プ径が小さくなって巻き付いて上方への移動ができなく
なる。したがって、ワイヤ送給ができなくなって溶接が
停止する。内筒6に使用する段ボール用ライナの厚さが
1.5mmを超えると、内筒6が変形しなくなるので、
複数のループが引き出された場合、ループ径が小さくな
って内筒6に巻き付いて上方への円滑な移動ができなく
なる。したがって、溶接機のワイヤ送給装置において大
きな抵抗となり、ワイヤ送給速度が一定とならず溶接ア
ークが不安定となったり、ワイヤ送給ができなくなって
溶接が停止する場合がある。
If the thickness of the corrugated cardboard liner used for the inner cylinder 6 is less than 0.8 mm, the inner cylinder 6 is partially tightened and deformed by the plurality of loops drawn out, and the loop diameter becomes small. It cannot be moved upward due to winding. Therefore, the wire cannot be fed and the welding stops. If the thickness of the cardboard liner used for the inner cylinder 6 exceeds 1.5 mm, the inner cylinder 6 will not be deformed,
When a plurality of loops are pulled out, the loop diameter becomes small, and the loops are wound around the inner cylinder 6 and cannot be smoothly moved upward. Therefore, a large resistance is generated in the wire feeding device of the welding machine, and the wire feeding speed may not be constant, and the welding arc may be unstable, or the wire feeding may not be performed, and the welding may be stopped.

【0012】次に、内筒6に使用する段ボール用ライナ
の秤量は400g/m2 以上としているので、複数のル
ープが引き出されて内筒6が変形した場合も、複数のル
ープがワイヤ取り出し装置または取り出し案内部材に導
かれて定常の状態になると円筒状に速やかに復元する。
また、引き出された複数のループによって絞られても亀
裂が生じることがない。したがって、引き出された複数
のループは内筒6に巻き付くことなく、その表面を抵抗
なく滑って上昇するから、円滑に引き出すことができ
る。
Next, since the weighing of the cardboard liner used for the inner cylinder 6 is set to 400 g / m 2 or more, even when a plurality of loops are pulled out and the inner cylinder 6 is deformed, the plurality of loops are connected to the wire take-out device. Alternatively, when it is guided by the take-out guide member and becomes a steady state, it is quickly restored to a cylindrical shape.
Further, no crack is generated even if the plurality of loops are drawn out. Therefore, the plurality of loops that are pulled out are not wound around the inner cylinder 6 and slide up on the surface without resistance, so that the loops can be pulled out smoothly.

【0013】内筒6に使用する段ボール用ライナの秤量
が400g/m2 未満であると、引き出された複数のル
ープによって内筒6が部分的に締め付けられて変形しす
ぎ、ループが巻き付いて上方への移動ができなくなる。
また、内筒6に亀裂が生じて巻き付いたループが亀裂に
引っかかり、上方への移動ができなくなる。したがっ
て、溶接機のワイヤ送給装置において大きな抵抗とな
り、ワイヤ送給ができなくなって溶接が停止する場合が
ある。
If the weight of the cardboard liner used for the inner cylinder 6 is less than 400 g / m 2 , the inner cylinder 6 is partially tightened by the plurality of pulled-out loops and deformed excessively, and the loops are wound around You cannot move to.
Further, a crack is formed in the inner cylinder 6 and a loop wound around the inner cylinder 6 is caught by the crack, so that the inner cylinder 6 cannot be moved upward. Therefore, a large resistance is caused in the wire feeding device of the welding machine, and the wire feeding may not be performed, and the welding may be stopped.

【0014】なお、内筒6に使用する段ボール用ライナ
の秤量の上限は、変形のし易さから460g/m2 以下
であることが好ましい。また、内筒6に使用する段ボー
ル用ライナは、縦方向を垂直としてペイル容器に固設し
て、該縦方向の引張強さは3N以上であることが好まし
い。なお、本発明にいう段ボール用ライナの秤量は、J
IS P8124に準じて測定した値をいう。
The upper limit of the weight of the cardboard liner used for the inner cylinder 6 is preferably 460 g / m 2 or less from the viewpoint of easy deformation. The cardboard liner used for the inner cylinder 6 is preferably fixed to a pail container with the vertical direction being vertical, and the tensile strength in the vertical direction is preferably 3 N or more. The weighing of the cardboard liner according to the present invention is J
A value measured according to ISP8124.

【0015】[0015]

【実施例】外筒外径510mm、高さ820mm(A)
と、外筒外径650mm、高さ770mm(B)の2種
類のペイル容器に、表1に示す厚さおよび秤量を変えた
各種段ボール用ライナ製の内筒をペイル容器底部に固設
して、ワイヤ径1.2mmのソリッドワイヤ(JIS
Z3312 YGW11)を、ループ状に1周回当たり
360°捩りながら、外筒と内筒との隙間に100kg
積層して押え板を載置した。
[Example] Outer cylinder outer diameter 510 mm, height 820 mm (A)
And two types of bail containers having an outer cylinder outer diameter of 650 mm and a height of 770 mm (B), and various types of corrugated cardboard liner inner cylinders having different thicknesses and weighings as shown in Table 1 were fixed to the bottom of the pail container. , A solid wire with a wire diameter of 1.2 mm (JIS
Z3312 YGW11) is twisted 360 ° per loop in a loop, and 100 kg is inserted into the gap between the outer cylinder and the inner cylinder.
The layers were stacked and the presser plate was placed.

【0016】それぞれの試験例について、溶接用ワイヤ
を積層体と内筒との間の円柱状空洞に5ループ引き出
し、ワイヤ取り出し案内部材を介して溶接装置により下
記溶接条件で3分間溶接して、溶接用ワイヤの取り出し
状態を調べる作業を10回繰り返して行った。その結果
も表1に示す。 溶接電流 :300A 溶接電圧 :30V 溶接速度 :30cm/min シールドガス:CO2 20リットル/分 溶接方法 :ビードオンプレート
For each of the test examples, a welding wire was drawn out into a cylindrical cavity between the laminate and the inner cylinder by five loops, and was welded for 3 minutes by a welding device through a wire take-out guide member under the following welding conditions. The operation of checking the state of taking out the welding wire was repeated 10 times. Table 1 also shows the results. Welding current: 300 A Welding voltage: 30 V Welding speed: 30 cm / min Shielding gas: CO 2 20 liter / min Welding method: Bead-on-plate

【0017】[0017]

【表1】 [Table 1]

【0018】表1中の試験 No.1〜6が本発明例、試験
No.7〜12が比較例である。本発明例である試験 No.
1〜6は、内筒に使用した段ボール用ライナの厚さおよ
び秤量が適正であるため、引き出された複数のループは
内筒に巻き付くが、内筒の外周長が先端部になるほど小
となるように変形して、巻き付いた複数のループは内筒
の外面を滑って上昇し、円滑に引き出すことができた。
また、複数のループの引き出しが完了して定常の状態に
なると、変形した内筒は円筒状に速やかに復元した。さ
らに、変形した時の内筒に亀裂が生じることもなかっ
た。
Test Nos. 1 to 6 in Table 1 are examples of the present invention and tests
Nos. 7 to 12 are comparative examples. Test No.
In the case of 1 to 6, since the thickness and weighing of the cardboard liner used for the inner cylinder are appropriate, the plurality of loops pulled out are wound around the inner cylinder, but are smaller as the outer peripheral length of the inner cylinder becomes the leading end. As a result, the wound loops could slide up the outer surface of the inner cylinder and be pulled out smoothly.
In addition, when the extraction of the plurality of loops was completed and a steady state was reached, the deformed inner cylinder was quickly restored to a cylindrical shape. Further, no crack was generated in the inner cylinder when deformed.

【0019】比較例中、試験 No.7および No.10は、
内筒に使用する段ボール用ライナの厚さが薄いため、引
き出された複数のループによって内筒が部分的に締め付
けられ、変形しすぎて上方への移動ができなくなりワイ
ヤ送給が停止した。試験 No.9および No.11は、内筒
に使用する段ボール用ライナの厚さが厚いいため内筒が
変形せず、ループ径が小さくなり内筒に巻き付いて、上
方への円滑な移動ができなくなって送給が不安定となっ
た。試験 No.10および No.12は、内筒に使用する段
ボール用ライナの秤量が低いため、複数のループによっ
て内筒が部分的に締め付けられて変形しすぎ、ループが
巻き付いて送給が停止した。また、試験 No.12は内筒
に亀裂が生じた。
In the comparative examples, tests No. 7 and No. 10
Since the thickness of the corrugated cardboard liner used for the inner cylinder was thin, the inner cylinder was partially tightened by the plurality of loops that were pulled out, was too deformed to move upward, and the wire feeding was stopped. In Tests No. 9 and No. 11, the thickness of the corrugated cardboard liner used for the inner cylinder was large, so the inner cylinder did not deform, the loop diameter became smaller, and it wrapped around the inner cylinder. The feeding became unstable due to the inability to do so. In Tests No. 10 and No. 12, the weighing of the corrugated cardboard liner used for the inner cylinder was low, so the inner cylinder was partially tightened by multiple loops, deformed too much, and the loop was wrapped to stop feeding. . In Test No. 12, cracks occurred in the inner cylinder.

【0020】[0020]

【発明の効果】以上詳述したように、本発明の溶接用ワ
イヤの装填物によれば、ペイル容器に積層収納された溶
接用ワイヤを取り出す際、複数のループが引き出された
場合においても、溶接用ワイヤが内筒に巻き付くことな
く、円滑に取り出すことができる。
As described above in detail, according to the loading of the welding wire of the present invention, even when a plurality of loops are pulled out when the welding wire stacked and stored in the pail container is taken out. The welding wire can be smoothly taken out without winding around the inner cylinder.

【図面の簡単な説明】[Brief description of the drawings]

【図1】本発明の溶接用ワイヤの装填物を用いたワイヤ
の取り出し状態を示す断面図である。
FIG. 1 is a cross-sectional view illustrating a state in which a wire is taken out using a charge of a welding wire according to the present invention.

【図2】図1のA−A′を示す断面図である。FIG. 2 is a sectional view showing AA ′ of FIG. 1;

【図3】従来の溶接用ワイヤの装填物を示す断面図であ
る。
FIG. 3 is a cross-sectional view showing a conventional welding wire charge.

【図4】従来の溶接用ワイヤの取り出し状態を示す断面
図である。
FIG. 4 is a sectional view showing a state in which a conventional welding wire is taken out.

【符号の説明】[Explanation of symbols]

1:外筒 2:積層体 3:押さえ板 4:円柱状空洞 5:溶接用ワイヤ 6:内筒 7:ペイル容器 8:底部 1: outer cylinder 2: laminated body 3: holding plate 4: columnar cavity 5: welding wire 6: inner cylinder 7: pail container 8: bottom

Claims (1)

【特許請求の範囲】[Claims] 【請求項1】 ペイル容器を構成する外筒と該ペール容
器の底部に固設された内筒との間にループ状に積層収納
した捩り入り溶接用ワイヤの装填物において、内筒は、
その厚さが0.8〜1.5mmで、かつ秤量が400g
/m2 以上の段ボール用ライナであり、捩り入り溶接用
ワイヤを装填したことを特徴とする溶接用ワイヤの装填
物。
1. A torsion-welding wire wire loaded and stored in a loop between an outer cylinder constituting a pail container and an inner cylinder fixed to the bottom of the pail container.
The thickness is 0.8-1.5mm and the weight is 400g
/ M 2 or more, which is a liner for corrugated cardboard, wherein a wire for torsion welding is loaded.
JP2000133835A 2000-05-02 2000-05-02 Welding wire charged article Withdrawn JP2001314968A (en)