DE1931420B1 - Use of a steel that has been vacuum-treated in the liquid state as a dynamo tape - Google Patents

Use of a steel that has been vacuum-treated in the liquid state as a dynamo tape

Info

Publication number
DE1931420B1
DE1931420B1 DE19691931420D DE1931420DA DE1931420B1 DE 1931420 B1 DE1931420 B1 DE 1931420B1 DE 19691931420 D DE19691931420 D DE 19691931420D DE 1931420D A DE1931420D A DE 1931420DA DE 1931420 B1 DE1931420 B1 DE 1931420B1
Authority
DE
Germany
Prior art keywords
steel
treated
rolled
vacuum
less
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
DE19691931420D
Other languages
German (de)
Inventor
Dr-Ing Schmithals Peter Ulrich
Dr-Ing Grasshoff Hans Wilhelm
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Hoesch AG
Original Assignee
Hoesch AG
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Hoesch AG filed Critical Hoesch AG
Publication of DE1931420B1 publication Critical patent/DE1931420B1/en
Pending legal-status Critical Current

Description

Es ist bekannt, Dynamoband mit Ummagnetisie- , rungsverlusten von 2,5 bis 4,0 W/kg bei Wechselfeldmagnetisierungen von 10 kG (50 Hz) mit einer Dicke von 0,35 bis 1,0 mm aus Stahl mit einem Siliziumgehalt von 1,0 bis 2,0%, einem Ausgangskohlenstoff gehalt von mehr als 0,015% und teilweise mit einem Aluminiumgehalt von 0,10 bis 0,50% herzustellen. Das Band oder Blech wird dazu warm- und kaltgewalzt und anschließend entkohlend und rekristallisierend entweder im Durchlaufofen, Kastenofen oder auch in einem sogenannten' Open-Coil-Haubenglühofen geglüht. Nachteilig bei diesen bekannten Verfahren sind · die im wesentlichen durch die Legierungen mit Silizium und/oder Aluminiumrbedingten niedrigen magnetischen Induktionswerte bei allen-Feldstärken und Frequenzen der erzeugten Dynamobleche oder -bänder.It is known that dynamo tape with magnetic reversal losses of 2.5 to 4.0 W / kg with alternating field magnetizations of 10 kG (50 Hz) with a thickness of 0.35 to 1.0 mm made of steel with a silicon content from 1.0 to 2.0%, a starting carbon content of more than 0.015% and partly with an aluminum content from 0.10 to 0.50%. The strip or sheet is hot and cold rolled for this purpose and then decarburizing and recrystallizing either in a continuous furnace, box furnace or in annealed in a so-called 'open coil hood annealing furnace. Disadvantages of these known processes are that they are essentially caused by the alloys with silicon and / or aluminum-related low magnetic induction values at all field strengths and frequencies of the dynamo sheets or strips produced.

Es ist ferner bekannt (vgl. Sam-arin, »Physikalisch-chemische Grundlagen der Desoxydation von Stahl«, 1960), Transformatorenstahl mit Si-Gehalten von etwa 3 % in einem Vakuumofen herzustellen und das zwischengeglühte, gewalzte Band einer Schlußglühung zu unterziehen. Die Wattverluste (W/kg) werden durch diese Behandlung gegenüber einem im herkömmlichen Induktionsofen hergestellten Stahl erniedrigt und die Werte der magnetischen Sättigung erhöht. Bekannt ist weiterhin ein Verfahren zur Herstellung von siliziumhaltigem Stahl für magnetische Zwecke (s. USA.-Patentschrift 2 287 467). Dieser bekannte Stahl hat einen Ausgangskohlenstoffgehalt von etwa 0,02 bis 0,06 % und einen Si-Gehalt bis zu 0,05 % herunter. Nach einem Zwischenglühen und dem Kaltwalzen wird das Entkohlungsglühen bei Temperaturen, von etwa 730.bis 9000C durchgeführt. Schließ- . lieh ist noch bekannt (s. Houdremont, »Hand-, buch der Sonderstahlkunde«, 1956, S. 1403), daß bei einem Stahl mit 0,003 bis 0,02% C, etwa 0,04 % Mn und etwa 0,01 % Si und einem steigenden Phosphorgehalt bis etwa 0,25% die Werte der mechanischen Eigenschaften, nämlich Dehnung, Zugfestigkeit und Streckgrenze ansteigen. Bekannt ist ferner aus der deutschen Offenlegungsschrift 1 433 799 ein Verfahren zur Herstellung von Schmiede- oder Flußeisen mit vef-' besserten elektrischen Eigenschaften, bei dem ein Stahl, der 0,03 bis 0,14% Kohlenstoff, 0,008 bis 0,15 % Phosphor, 0,38 bis 0,76% Mangan, höchstens 0,03% Schwefel und höchstens 0,02% Silizium enthält, nach einer Verarbeitung zu Blech, bestehend aus Warmwalzen, Aufspulen bei 649 bis 7040C, nachfolgendem Kaltreduzieren und .Entkehlen bei einer Temperatur ■ zwischen 621 und 7Q4°C auf einen Kohlenstoffgehalt von weniger als 0,008^Z0, Glühen bei einer Temperatur zwischen 816 und 843 0C und abschließendem Vergütungswalzen des ^Bandes, -verbesserte magnetische Eigenschaften aufwejjst. In nachteiliger Weise werdenbei diesem bekannten"Verfahren ebenso wie bei dem aus der deutschen Auslegeschrift 1 261146 bekannten Verfahren eine zusätzliche Glühung und eine zusätzliche Verformung durchgeführt, um Kernverluste von etwa 7 bzw. 9 W/kg bei 50 Hz zu erreichen.It is also known (cf. Sam-arin, "Physikalisch -chemische bases der Deoxydation von Stahl", 1960) to produce transformer steel with Si contents of about 3% in a vacuum furnace and to subject the intermediate annealed, rolled strip to a final anneal. The watt losses (W / kg) are reduced by this treatment compared to steel produced in a conventional induction furnace and the values of the magnetic saturation are increased. A method for producing silicon-containing steel for magnetic purposes is also known (see US Pat. No. 2,287,467). This known steel has an initial carbon content of about 0.02 to 0.06% and an Si content down to 0.05%. After an intermediate annealing and cold rolling, decarburization annealing at temperatures is carried out from about 900 0 C 730.bis. Closing. borrowed is still known (see Houdremont, "Hand-, buch der Sonderstahlkunde", 1956, p. 1403) that in a steel with 0.003 to 0.02% C, about 0.04% Mn and about 0.01% Si and an increasing phosphorus content of up to about 0.25%, the values of the mechanical properties, namely elongation, tensile strength and yield point, increase. Also known from German Offenlegungsschrift 1 433 799 is a process for the production of wrought iron or fluoro iron with improved electrical properties, in which a steel containing 0.03 to 0.14% carbon, 0.008 to 0.15% phosphorus , 0.38 to 0.76% manganese, a maximum of 0.03% sulfur and a maximum of 0.02% silicon, after processing into sheet metal, consisting of hot rolling, coiling at 649 to 704 0 C, subsequent cold reduction and decalcifying at ■ a temperature between 621 and 7Q4 ° C on a carbon content of less than 0.008 ^ Z 0, annealing aufwejjst at a temperature of 816-843 0 C and abschließendem temper rolling the strip ^, -improved magnetic properties. Disadvantageously, in this known "method, as in the method known from German Auslegeschrift 1 261146, additional annealing and additional deformation are carried out in order to achieve core losses of about 7 and 9 W / kg at 50 Hz, respectively.

Der Erfindung liegt die Aufgabe zugrunde, einen Stahl anzugeben, der bei gleichen Ummagnetisierungsverlusten wie die mit Si und/oder Al legierten Stähle diesen gegenüber erhöhte magnetische Induktionswerte aufweist. Eine weitere Aufgabe der Erfindung ist es, gegenüber den bekannten Verfahren zur Herstellung von Dynamoband ein vereinfachtes Verfahren anzugeben.The invention is based on the object of specifying a steel which, with the same core losses like the steels alloyed with Si and / or Al, compared to these, increased magnetic induction values having. Another object of the invention is compared to the known processes for the production of Dynamo tape to specify a simplified procedure.

Diese Aufgaben werden gelöst durch die Verwendung eines im flüssigen Zustand vakuumbehandelten Stahls bestehend aus weniger als 0,015% Kohlenstoff, 0,050 bis 0,250% Phosphor, Rest Eisen mit den herstellungsbedingten Verunreinigungen, der warmgewalzt, gebeizt, kaltgewalzt und anschließend jm Durchlaufofen bei einer Temperatur von 750 bis 11000C 2 bis 7 Minuten lang auf weniger als 0,010% Kohlenstoff entkohlt worden ist, als Dynamoband mit einem Ummagnetisierungsverlust von 2,5 bis 4,0 W/kg bei einer Wechselfeldmagnetisierung von 10 kG (50 Hz) und einer gegenüber mit Silizium legiertem Stahl erhöhten magnetischen Induktion von mindestens 500 bis 1000 G bei Wechselfeldstärken zwischen 5 und 300 A/cm (50 Hz). An Stelle der Behandlung im Durchlaufofen kann der vorerwähnte Stahl zweckmäßigerweise auch in einem geschlossenen Ofenraum stationär bei 650 bis 950° C 30 Minuten bis 24 Stunden lang auf weniger als 0,01% Kohlenstoff geglüht werden.These objects are achieved by using a steel that has been vacuum-treated in the liquid state and consists of less than 0.015% carbon, 0.050 to 0.250% phosphorus, the remainder iron with the production-related impurities, which is hot-rolled, pickled, cold-rolled and then in a continuous furnace at a temperature of 750 to 1100 0 C has been decarburized to less than 0.010% carbon for 2 to 7 minutes, as a dynamo tape with a magnetic reversal loss of 2.5 to 4.0 W / kg with an alternating field magnetization of 10 kG (50 Hz) and one alloyed with silicon Steel increased magnetic induction of at least 500 to 1000 G with alternating field strengths between 5 and 300 A / cm (50 Hz). Instead of being treated in a continuous furnace, the above-mentioned steel can expediently also be annealed to less than 0.01% carbon in a stationary furnace at 650 to 950 ° C. for 30 minutes to 24 hours.

In zweckmäßiger Weise ist ferner vorgesehen, daß bei einem Phosphorgehalt von weniger als 0,050% Mangan in Höhe vpn 0,50 bis 1,10 % zugesetzt wird. Sollen die erfindungsgemäßen Eigenschaften des Stahls weiter verbessert werden, so ist eine Desoxydation mit bis zu 0,80% Mangan und/oder bis zu 0,50% Silizium und/oder bis zu 0,10 % Aluminium mit Vorteil möglich.Appropriately, it is also provided that with a phosphorus content of less than 0.050% Manganese is added in the amount of 0.50 to 1.10%. Shall the properties of the steel according to the invention can be further improved, so is a deoxidation with up to 0.80% manganese and / or up to 0.50% silicon and / or up to 0.10% aluminum is advantageously possible.

Die Vorteile des erfindungsgemäß zu verwendenden Stahls sind insbesondere darin zu sehen, daß auf einfache Weise gleichzeitig die Magnetisierungs- oder In-.duktionswerte bei den genannten Ummagnetisierungs-' Verlusten um mindestens 500 und bis zu 2C0O G gegenüber üblichen mit Silizium legierten Stählen gesteigert werden können, wodurch die Leistung der aus diesem Werkstoff gefertigten elektrischen Geräte ohne Ansteigen des Einsatzgewichtes erhöht wird. Da die Leistung von Elektrogeräten, z. B. das Drehmoment von Elektromotoren, bei bestimmten Drehzahlen wesentlich durch die magnetischen Induktionswerte beeinflußt wird, sind Dynamobänder, die bei gleichen Ummagnetisierungsverlusten höhere magnetische Induktionswerte aufweisen, gegenüber den bekannten mit Silizium legierten Bändern vorzuziehen. Neben einer sehr guten Alterungsbeständigkeit weist der Stahl ein rein ferritisches Gefüge mit geringen Resten Tertiärzementit sowie ohne Nachwalzung eine Zugfestigkeit von 35 bis etwa 50 kp/mm2 auf, so daß eine erhöhte Gratbildung und ein Schmieren beim Stanzen verhindert und gute Werkzeugstandzeiten gewährleistet werden.The advantages of the steel to be used according to the invention are to be seen in the fact that the magnetization or induction values can be increased in a simple manner at the same time with the mentioned magnetic reversal losses by at least 500 and up to 20,000 compared to conventional silicon-alloyed steels , whereby the performance of the electrical devices made of this material is increased without increasing the operating weight. As the performance of electrical appliances, e.g. B. the torque of electric motors is significantly influenced by the magnetic induction values at certain speeds, dynamo tapes, which have higher magnetic induction values with the same magnetic reversal losses, are to be preferred over the known silicon-alloyed tapes. In addition to very good aging resistance, the steel has a purely ferritic structure with small amounts of tertiary cementite and, without re-rolling, a tensile strength of 35 to about 50 kp / mm 2 , so that increased burr formation and smearing during punching are prevented and good tool life is guaranteed.

Im folgenden werden die Herstellung des erfindungsgemäß zu verwendenden Stahls sowie die dabei erzielten Eigenschaften an Hand von Ausführungsbeispielen näher erläutert. In the following the production of the invention Steel to be used and the properties achieved are explained in more detail on the basis of exemplary embodiments.

Drei verschiedene Stähle A,' B und C wurden im Siemens-Martin-Qfen (A, B) bzw. Induktionsofen (C) erschmolzen und anschließend in einer Vakuumanlage im flüssigen Zustand behandelt. Die chemische Zusammensetzung der Stähle nach der Vakuumbehandlung zeigt Tabelle 1.Three different steels A, 'B and C were in the Siemens-Martin-Qfen (A, B) and induction furnace (C) melted and then treated in a vacuum system in the liquid state. The chemical The composition of the steels after the vacuum treatment is shown in Table 1.

Tabelle 1Table 1 Stahl A Steel A CVoCVo SiVoSiVo MnVoMnVo P%P% ,. s Vo,. s Vo NVoNVo AlVoAlVo Stahl B Steel B 0,007
0,008
0,015
0.007
0.008
0.015
0,02
<0,01
<0,01
0.02
<0.01
<0.01
0,34
0,33
0,46
0.34
0.33
0.46
0,148
0,207
0,140
0.148
0.207
0.140
0,014
0,016
0,022
0.014
0.016
0.022
0,003
0,003
0,006
0.003
0.003
0.006
0,006
< 0,003
< 0,003
0.006
<0.003
<0.003
Stahl C Steel C

Nach, dem Warmwalzen der Stähle A und B auf die Abmessung 1000 · 2 mm wurde das Band in 15%iger Schwefelsäure bei etwa 980C gebeizt, auf einer fünfge rüstigen Tandemstraße an die Abmessung 1000 · 0,5 mm kaltgewalzt und auf 980 · 0,50 mm besäumt. Der Stahl C wurde an die Abmessung 110 · 2,0 mm auf einer kontinuierlichen Mittelbandstraße warmgewalzt und nach der gleichen Beizung an 110 · 0,50mm auf einem Duo-Gerüst in fünf Stichen kaltgewalzt. Nach der entkohlenden Rekristallisationsglühung im Durchlaufofen bei 850 bis 900° C und Verweilzeiten zwischen 3 und 7 Minuten ergaben sich die in Tabelle 2 für 850°C und in Tabelle 3 für 900°C angegebenen, aus Längs- und Querproben gemittelten Werte der Ummägnetisierungsverluste F 100)5 in W/kg bei einer Wechselfeldmagnetisierung von 10 kG.After hot rolling of the steels A and B, the tape in 15% sulfuric acid was mm to the dimension of 1000 x 2 stained at about 98 0 C, at a fünfge vigorous tandem mill to the dimensions of 1000 x 0.5 cold rolled mm and 980 · Trimmed 0.50 mm. Steel C was hot-rolled to dimensions 110 x 2.0 mm on a continuous medium strip mill and, after the same pickling, was cold-rolled to 110 x 0.50 mm on a two-high stand in five passes. After the decarburizing recrystallization annealing in a continuous furnace at 850 to 900 ° C and residence times between 3 and 7 minutes, the values of the re-magnetization losses F 10 given in Table 2 for 850 ° C and in Table 3 for 900 ° C, averaged from longitudinal and transverse samples, resulted 0) 5 in W / kg with an alternating field magnetization of 10 kG.

Tabelle 2Table 2 V
4 Min.
V
4 min.
erweüzeit
5 Min. 16 Min.
awakening
5 min. 16 min.
3,7
3,3
n.b.·
3.7
3.3
nb ·
7 Min:7 min:
3 Min.3 min. 3,8
3,3
3,75
3.8
3.3
3.75
3,8
3,4
3,6
3.8
3.4
3.6
; 3,5-
.3,2
3,3 :
; 3.5-
.3.2
3.3:
Stahl A Steel A 3,9
3,5
4,0
3.9
3.5
4.0
Stahl B Steel B Stahl C Steel C

Tabelle 3Table 3

3 Min.3 min. Verweilze
4 Min. 15 Min..
Linger
4 min. 15 min.
3,4
3,1
3,85
3.4
3.1
3.85
it
6 Min.
it
6 min.
7.Min.7 min.
Stahl A Steel A 3,4
3,5
.4,0
3.4
3.5
.4.0
3,3
3,2
3,9
3.3
3.2
3.9
3,4
3,1
n:b.
3.4
3.1
n: b.
3,3
3,1
3,8
3.3
3.1
3.8
Stahl B. Steel B. StahlC SteelC

Die Restkohlenstoffgehalte in Prozent der Stähle nach der rekristallisierenden Entkohlungsglühung in iner Atmosphäre aus;teilverbranntem Ferngas mit 12% H2, T0J0CO, 6% CO2, Rest N2 und einem Tau-The residual carbon content in percent of the steels after the recrystallizing decarburization annealing in an inner atmosphere ; partially burned gas with 12% H 2 , T 0 J 0 CO, 6% CO 2 , remainder N 2 and a dew

punkt von +200C zeigt Tabelle 4.point of +20 0 C is shown in Table 4.

TabelleTabel

Restkohlenstoffgehalte (%) nach Entkohlung und Rekristallisation bei 850°C/4Min. I 850°C/7Min. I 900°C/4Min. I 900°C/7Min.Residual carbon content (%) after decarburization and recrystallization 850 ° C / 4 min. I 850 ° C / 7 min. I 900 ° C / 4 min. I 900 ° C / 7 min.

Stahl A
Stahl B
StahlC
Steel A
Steel B
SteelC

0,002
0,003
0,0095
0.002
0.003
0.0095

0,001
0,002
0,007
0.001
0.002
0.007

0,002 0,001 0,0100.002 0.001 0.010

0,001 0,001 0,0090.001 0.001 0.009

Die nach der Entkohlung und Rekristallisierung bei 8500C in 4 Minuten erzielten magnetischen Induktionswerte sind als Mittelwerte aus Längs- und Querproben in Tabelle 5 angegeben. Zum Vergleich ist ein Stahl D mit 0,92 °/0 Si und 0,08 % Al und ein Stahl E mit 1,0% Si und 0,20% Al, deren Ummägnetisierungsverluste V 100j5 mit 2,6 W/kg gemessen wurden, angegeben.The obtained after decarburization and recrystallization at 850 0 C in 4 minutes magnetic induction values are given as mean values of longitudinal and transverse test pieces in Table 5 below. For comparison, a steel D 0.92 ° / 0 Si and 0.08% Al and a steel E containing 1.0% Si and 0.20% Al whose Ummägnetisierungsverluste V 10 0j5 kg measured at 2.6 W / were specified.

Bei einer Glühbehandlung bei 9000C in 4 Minuten sind die Unterschiede in den Meßwerten kaum festzustellen. In the case of an annealing treatment at 900 ° C. for 4 minutes, the differences in the measured values can hardly be ascertained.

Tabelle 5Table 5

B 25B 25 B 50B 50 BlOOBlOO B 300B 300 Stahl A Steel A 16,9
17,2
n.b.
16,5
16,4
16.9
17.2
nb
16.5
16.4
18,4
18,8
n.b.
17,4
17,2
18.4
18.8
nb
17.4
17.2
18,9
19,3
19,0
18,4
18,2
18.9
19.3
19.0
18.4
18.2
19,9
20,3
n.b.
19,4
19,2
19.9
20.3
nb
19.4
19.2
Stahl B .. Steel B .. Stahl C Steel C Stahl D Steel D Stahl E Steel E.

Dynamobänder mit einem Ummagnetisierungsverlust von 2,3 bis 3,6 W/kg bei Wechselfeldmagnetisierungen (50 Hz) von 10 kG (vgl. Tabelle 6).Dynamo tapes with a core loss of 2.3 to 3.6 W / kg with alternating field magnetizations (50 Hz) of 10 kG (see Table 6).

Tabelle 6Table 6 40 Güte40 goodness Band
oder
Blechdicke
tape
or
Sheet thickness
Um-Around- Magnetische Induktionen
(kG) mind.
Magnetic inductions
(kG) at least
B 50B 50 BlOOBlOO B 300B 300
magneti-
sierungs-
verlust
magnetic
ization
loss
16,416.4 17,517.5 20,120.1
(mm)(mm) FlOFlO B 25B 25 16,516.5 17,617.6 20,020.0 Dyba 23Dyba 23 0,500.50 (W/kG)(W / kG) 15,315.3 16,616.6 17,717.7 19,819.8 45 Dyba2645 Dyba26 0,500.50 2,32.3 15,515.5 16,816.8 17,817.8 19,719.7 Dyba 30Dyba 30 0,500.50 2,62.6 15,615.6 Dyba 36Dyba 36 0,500.50 3,03.0 15,815.8 3,63.6

Ein Vergleich der gemessenen Werte mit den Mindestwerten für die magnetische Induktion nach dem neuen Vorschlag der DIN 46 400 für kaltgewalzte zeigt, daß das kaltgewalzte und im Durchlaufofen einer Schlußglühung unterzogene Stahlband bzw. -blech nach der Erfindung die nach der DIN-Norm angegebenen Mindestwerte der magnetischen Induktionen um 200 bis 2000 G überschreitet.A comparison of the measured values with the minimum values for magnetic induction according to the new proposal of DIN 46 400 for cold-rolled shows that the cold-rolled steel strip or steel strip subjected to final annealing in a continuous furnace sheet according to the invention, the minimum values of the magnetic induction specified in accordance with the DIN standard exceeds 200 to 2000 G.

Die nach der Entkohlung und Rekristallisierung bei 850 bzw. 9000C in 4 Minuten erreichten mechanischen Eigenschaften zeigt Tabelle 7.The mechanical properties achieved in 4 minutes after decarburization and recrystallization at 850 and 900 ° C. are shown in Table 7.

TabelleTabel

Mechanische Eigenschaften nach Entkohlung und RekristallisierungMechanical properties after decarburization and recrystallization

Streckgrenze
as (kp/mm2)
Stretch limit
a s (kp / mm 2 )

bei 850° G/4 Min.
Zugfestigkeit
aB (kp/mm2) Bruchdehnung
c, (%)
at 850 ° G / 4 min.
tensile strenght
a B (kp / mm 2 ) elongation at break
c, (%)

Streckgrenze
Cs (kp/mm2)
Stretch limit
Cs (kp / mm 2 )

bei 900° C/4 Min. Zugfestigkeit Ob (kp/mm2)at 900 ° C / 4 min. tensile strength Ob (kp / mm 2 )

BruchdehnungElongation at break

Stahl A.
Stahl B.
StahlC
Steel A.
Steel B.
SteelC

28,8
30,9
30,8
28.8
30.9
30.8

38,9
41,1
39,0 59,5
47,5
52,5
38.9
41.1
39.0 59.5
47.5
52.5

29,3
29,8
31,2
29.3
29.8
31.2

39,7 39,8 39,539.7 39.8 39.5

50,5 50,5 52,550.5 50.5 52.5

Die ermittelten, mechanischen Eigenschaften, insbesondere die Zugfestigkeit, ergeben bei dem erfindungsgemäßen Stahl bei entsprechender Einstellung des Spaltes ein gutes Stanzverhalten. Im übrigen zeigten die Stähle nach der Entkohlung ein rein ferritisches Gefiige mit geringen Resten an Tertiärzementit und einer ASTM-KorngrÖße zwischen 5 bis 8 sowie einen guten nichtmetallischen Reinheitsgrad.The mechanical properties determined, in particular the tensile strength, result in the steel according to the invention with the appropriate setting of the gap a good punching behavior. Otherwise, the steels showed a purely ferritic quality after decarburization Vessels with small residues of tertiary cementite and an ASTM grain size between 5 and 8 as well a good non-metallic degree of purity.

Claims (4)

Patentansprüche:Patent claims: 1. Verwendung eines im flüssigen Zustand vakuumbehandelten Stahls, bestehend aus weniger als 0,015 0/0 Kohlenstoff, 0,050 bis 0,250% Phosphor, Rest Eisen mit den herstellungsbedingten Verunreinigungen, der warmgewalzt, gebeizt, kaltgewalzt und anschließend im Durchlaufofen bei einer Temperatur von 750 bis HOD0C 2 bis 7 Minuten lang auf wenigsr als 0,010 % Kohlenstoff entkohlt worden ist, als Dynamoband mit einem Ummagnetisierungsverlust von 2,5 bis 4,0 W/kg bei einer Wechselfeldmagnetisierung von 10 kG (50 Hz) und einer gegenüber einem üblichen mit Silizium legierten Stahl erhöhten magnetischen Induktion von mindestens 500 bis 1000 G bei Wechselfeldstärken zwischen 5 bis 300 A/cm (50Hz)1. Use of a vacuum-treated in the liquid state steel consisting of less than 0.015 0/0 carbon, 0.050 to 0.250% phosphorus residue iron with impurities resulting from manufacture, the hot rolled, pickled, cold rolled, and then in a continuous furnace at a temperature of 750 to HOD 0 C has been decarburized for 2 to 7 minutes to less than 0.010% carbon, as a dynamo tape with a core loss of 2.5 to 4.0 W / kg with an alternating field magnetization of 10 kG (50 Hz) and one compared to a conventional one with silicon Alloy steel increased magnetic induction of at least 500 to 1000 G with alternating field strengths between 5 to 300 A / cm (50Hz) 2. Verwendung eines im flüssigen Zustand vakuumbehandelten Stahls der Zusammensetzung nach Anspruch 1, der warmgewalzt, gebeizt, kaltgewalzt und anschließend in einem geschlossenen Ofenraum stationär bei 650 bis 9500C 30 Minuten bis 24 Stunden lang auf weniger als 0,01 % Kohlenstoff geglüht wird, zu dem Zweck nach Anspruch 1.2. Use of a steel, vacuum-treated in the liquid state, of the composition according to claim 1, which is hot-rolled, pickled, cold-rolled and then stationary in a closed furnace chamber at 650 to 950 ° C. for 30 minutes to 24 hours to less than 0.01% carbon , for the purpose of claim 1. 3. Verwendung eines Stahls, bestehend aus weniger als 0,05 % Phosphor, 0,5 bis 1,1 % Mangan, Rest Eisen mit den herstellungsbedingten Verunreinigungen, behandelt nach Anspruch 1 oder 2, zu dem Zweck nach Anspruch 1.3. Use of a steel consisting of less than 0.05% phosphorus, 0.5 to 1.1% manganese, The remainder of iron with the production-related impurities, treated according to claim 1 or 2, for the purpose of claim 1. 4. Verwendung eiaes Stahls der Zusammensetzung nach Anspruch 1 oder 3, der bis zu 0,8 % Mangan und/oder bis zu 0,5 % Silizium und/oder bis zu 0,1 % Alumioium enthält, behandelt nach Anspruch 1 oder 2, zu dem Zweck nach Anspruch 1.4. Use eiaes steel of the composition according to claim 1 or 3, of up to 0.8% manganese and / or up to 0.5% silicon and / or up to 0.1% of Al to ioium, treated according to claim 1 or 2, for the purpose of claim 1.
DE19691931420D 1969-06-20 1969-06-20 Use of a steel that has been vacuum-treated in the liquid state as a dynamo tape Pending DE1931420B1 (en)