CN1919954A - Antifriction repairing agent with natural minerals as main components, preparation method and application - Google Patents

Antifriction repairing agent with natural minerals as main components, preparation method and application Download PDF

Info

Publication number
CN1919954A
CN1919954A CN200510092996.4A CN200510092996A CN1919954A CN 1919954 A CN1919954 A CN 1919954A CN 200510092996 A CN200510092996 A CN 200510092996A CN 1919954 A CN1919954 A CN 1919954A
Authority
CN
China
Prior art keywords
antifriction
restoring agent
agent
main component
natural
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
CN200510092996.4A
Other languages
Chinese (zh)
Other versions
CN100497514C (en
Inventor
白志民
尤肃生
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Beijing Mo'an Tianjie Technology Co ltd
Original Assignee
Beijing Youyue Science & Technology Co ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Beijing Youyue Science & Technology Co ltd filed Critical Beijing Youyue Science & Technology Co ltd
Priority to CNB2005100929964A priority Critical patent/CN100497514C/en
Publication of CN1919954A publication Critical patent/CN1919954A/en
Application granted granted Critical
Publication of CN100497514C publication Critical patent/CN100497514C/en
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

The invention discloses an antifriction repairing agent with natural minerals as main components, which comprises the following components in parts by mass: natural serpentine mineral powder: 30-79.5 parts of nickel-containing compound: 0.5-1.5 parts of a surface modifier: 20 to 69.5 portions. The preparation method comprises the following steps: mixing the proportioned raw materials by a ball mill, homogenizing at the temperature of 70-80 ℃ for 18-24 hours, and grinding by the ball mill to obtain powder with the average particle size of 0.5-1.2 microns. The invention also discloses antifriction repair gel, antifriction repair lubricating grease and antifriction repair lubricating oil containing the antifriction repair agent. The antifriction repairing agent of the invention has good antifriction and repairing functions, can greatly prolong the service life of parts, and takes natural minerals as raw materials, and has simple processing technology and low cost.

Description

With the natural mineral is Antifriction restoring agent, preparation method and the application of main component
Technical field
The present invention relates to a kind of renovation agent, particularly a kind of is the Antifriction restoring agent of main component with the natural mineral, also relates to the preparation method of above Antifriction restoring agent, also relates to the application of above Antifriction restoring agent.
Background technology
Common Antifriction restoring agent, the mixture of synthetic or natural mineral normally, its composition are complicated, and complete processing is also complicated, so cost is higher.
Such as: China's application: disclose a kind of composition that friction pair is handled that is used in 008001330.6, comprised multiple oxide compound, and course of processing complexity, just can use after need dewatering to hydrous oxide.
China application: disclose a kind ofly in 02120826.3, comprised multi mineral, complicated component in the solid lubrication composition of handling with friction pair.
Summary of the invention
The present invention has overcome the shortcoming of Antifriction restoring agent course of processing complexity in the prior art, provides that a kind of what have high-quality antifriction, repair is the Antifriction restoring agent of main component with the natural mineral, and the preparation method of this Antifriction restoring agent also further is provided; Several application of this Antifriction restoring agent also further are provided.
In order to achieve the above object, of the present invention a kind of be the Antifriction restoring agent of main component with the natural mineral, comprise the component of following quality proportioning:
Natural serpentine minerals powder: 30~79.5 parts,
Nickel compound containing: 0.5~1.5 part,
Surface-modifying agent: 20~69.5 parts.
As a kind of preferred version, the composition that described natural serpentine contains is:
Mg 5-6Fe 0-1[Al 0-1Si 3-4]O 10(OH) 8
As further preferred version, the composition that described natural serpentine contains is:
K 0.02Fe 0.02Ca 0.06Mn 0.03Mg 5.69P 0.01Al 0.17Si 4.00O10(OH) 8
Above-mentioned natural serpentine minerals particles of powder diameter is preferred≤and 10 microns.
The mixture of one or more in the preferred following component of above-mentioned nickel compound containing: Ni (OH) 21/4H 2O, NiCl 26H 2O, Ni (NO 3) 26H 2O, or NiSO 46H 2O.This nickel compound containing mainly plays catalyst action, and Ni ion has wherein quickened the formation of composite ceramic layer under friction condition.
Described surface-modifying agent is one or more the mixture in the following component: Span60, Tween60 or Span80.It mainly acts on is that mineral dust is carried out surface modification, thereby improves the suspension stability of mineral dust.Above surface-modifying agent is existing procucts, and the chemical formula of Span60 can be C 24H 46O 6
The preparation method of above Antifriction restoring agent may further comprise the steps:
1, the raw material according to above-mentioned mass ratio carries out proportioning, mixes:
2, the raw material of said ratio is mixed back homogenizing processing 18~24 hours under 70~80 ℃ temperature through ball mill, obtain the powder of 0.5~1.2 micron of mean particle size again through ball mill grinding, promptly forming of the present invention is the Antifriction restoring agent of main component with the natural mineral.
More than be that the Antifriction restoring agent of main component is a raw material with the natural mineral, as application, can make multiple reparation product:
A. gel is repaired in antifriction: the above-mentioned Antifriction restoring agent of 60~70 mass parts mixes with the lubricating oil of 30~40 mass parts, stirs 2~3 hours under 70~80 ℃ of temperature, can obtain antifriction and repair gel.
These goods both can be applied directly to surfaces of metallic rubbing pairs, can be 1~2 to be that 98~99 industrial lubricant mixes the back and uses with mass parts by mass parts with this Antifriction restoring agent gel also.
B. lubricating grease is repaired in antifriction: the above-mentioned Antifriction restoring agent of 1~3 mass parts mixes with the industrial grease of 97~99 mass parts, stirs homogenizing and handle under chambers temp, can obtain antifriction and repair lubricating grease, and directly adding frictional interface can use.
C. lubricating oil is repaired in antifriction: the Antifriction restoring agent of 0.5~2 mass parts mixes with the industrial lubricant of 98~99.5 mass parts, stirs 2~3 hours under 70~80 ℃ of temperature, can obtain Antifriction restoring agent lubricating oil.
More than repair the product using method:
1, product being repaired in a certain proportion of antifriction, added the machine oiling system, is medium with the lubricant, carries it into the friction pair interface, makes surface of friction pair obtain modification and reparation in machine run;
2, when the machine disintegration is opened and inspect, directly be applied to damage parts or wear and tear overrun surface, repaired through the relative friction of certain hour;
3, also can be other methods of repairing by friction.
The beneficial effect of Antifriction restoring agent is:
1, to the effective antifriction reparation of element part, save energy and material meet the developing direction of recycling economy;
2, with the natural mineral be main raw material, add proper catalyst and surface-modifying agent and make the Antifriction restoring agent powder that composition is simple, with low cost, technology is simple;
3, can be made into the gel of different purposes or, be applicable to multiple occasion based on the broad variety product of lubricating grease or lubricating oil;
4, can utilize the operating mode of machine to realize selfreparing, need not cost of labor;
5,, belong to the Industrial products of environmental protection class based on natural matter.
Description of drawings
Fig. 1 illustrates the scanning electron microscope image of the Antifriction restoring agent of the embodiment of the invention.
Embodiment
With reference to following examples, will be described in detail embodiment of the present utility model.
Embodiment 1
Mix according to following mass fraction proportioning:
Natural serpentine minerals powder: K 0.02Fe 0.02Ca 0.06Mn 0.03Mg 5.69P 0.01Al 0.17Si 4.00O10(OH) 8Mineral dust 5.0kg
Ni(OH) 2·1/4H 2O 0.1kg
Span60 4.9kg
The raw material of said ratio is mixed back homogenizing under 75 ℃ of temperature through ball mill handled 20 hours, again through the Antifriction restoring agent powder of about 1.0 microns of ball mill grinding acquisition mean particle sizes.Fig. 1 illustrates the scanning electron microscope image of this Antifriction restoring agent.
With above-mentioned powder 0.08kg with after industrial lubricant 9.92kg mixes, under 75 ℃ of temperature, stirred 2 hours, obtain antifriction and repair lubricating oil.
Repairing lubricating oil with above-mentioned antifriction is that sample carries out four ball frictional experiments, and the result shows: this friction coefficient of lubricating oil reduces by 38% than base oil, and wear scar diameter reduces 25%.72 hours ring-mills decrease experiment and show that when being lubricant medium with this lubricating oil, the abrasion loss of friction pair in initial 2 hours just contrasts 50% of base oil friction pair; After 36 hours, the abrasion loss of using this antifriction to repair the friction pair of lubricating oil just contrasts 2% of base oil friction pair; After 72 hours, wearing and tearing no longer appear in friction pair, and its quality increases by 1 ‰ on the contrary.
Experiment shows that renovation agent of the present invention has tangible antifriction and repair to mechanical metallic rubbing pairs, has better industrial application prospect.
Because the natural serpentine minerals powder that present embodiment uses, thus its composition because the mineral products thing of different location and difference, wherein main component can be Mg 5-6Fe 0-1[Al 0-1Si 3-4] O 10(OH) 8, the less composition of other amounts can change by trace, but little to realizing purpose influence of the present invention.
Embodiment 2
The Antifriction restoring agent powder that embodiment 1 is made: 3.0kg with industrial lubricant: 2.0kg, stirred 2.5 hours under 75 ℃ of temperature, can obtain the Antifriction restoring agent gel.
After the railway locomotive overhaul, during ten thousand kilometers of about 5-6 of traveling, diesel engine of locomotive is carried out waterr rheostat test and machine oil chemical examination.According to the diesel engine state, be 98~99: 1~2 ratio in mass ratio with total oil mass of lubrication box and above-mentioned Antifriction restoring agent gel, add above-mentioned antifriction and repair gel.Add the back locomotive operation and extend to that the phase of repairing is that 600,000 kilometers time sides of traveling open and inspect test in two, and with one of the operation of carrying out existing maintenance procedure in repair the phase promptly 300,000 kilometers locomotive compare.The result shows: each compression pressure without combustion of diesel engine, explosion pressure and power and rational curve are all within range of normal value.Main friction pairs as the cylinder liner piston ring group, still maintains a good state.Its wear loss is lower than and does not add the antifriction renovation agent and only move i.e. 300,000 kilometers locomotive of the phase of repairing in one.For example, barrel wear average (with the increase variable quantity nominal of cylinder sleeve diameter): that add 600,000 kilometers of antifriction renovation agent travelings is 0.040mm; And do not add 300,000 kilometers of antifriction renovation agent travelings for 0.059mm.Piston ring side clearance: the 0.027mm that is that adds 600,000 kilometers of antifriction renovation agent travelings: the 0.053mm that is that does not add 300,000 kilometers of antifriction renovation agent travelings.Through 600,000 kilometers operation, the thickness of the piston ring that has and piston ring end gap clearance no change.Not only antifriction but also repairing effect is arranged of this explanation the present invention.The cylinder liner piston ring group is expected to prolong and uses 900,000 kilometers, promptly prolongs twice its work-ing life.Owing to repair number of times in reducing, prolong part work-ing life, can bring great economic benefit to railway enterprise.

Claims (13)

1, a kind of is the Antifriction restoring agent of main component with the natural mineral, comprises the component of following quality proportioning:
Natural serpentine minerals powder: 30~79.5 parts,
Nickel compound containing: 0.5~1.5 part,
Surface-modifying agent: 20~69.5 parts.
2, according to claim 1 is the Antifriction restoring agent of main component with the natural mineral, it is characterized in that, the composition that described natural serpentine contains is:
Mg 5-6Fe 0-1[Al 0-1Si 3-4]O 10(OH) 8
3, according to claim 2 is the Antifriction restoring agent of main component with the natural mineral, it is characterized in that, the composition that described natural serpentine contains is:
K 0.02Fe 0.02Ca 0.06Mn 0.03Mg 5.69P 0.01Al 0.17Si 40.0O 10(OH) 8
4, according to claim 1 is the Antifriction restoring agent of main component with the natural mineral, it is characterized in that, described natural serpentine minerals particles of powder diameter≤10 microns.
5, according to claim 1 is the Antifriction restoring agent of main component with the natural mineral, it is characterized in that, described nickel compound containing is one or more the mixture in the following component:
Ni (OH) 21/4H 2O, NiCl 26H 2O, Ni (NO 3) 26H 2O, or NiSO 46H 2O.
6, according to claim 1 is the Antifriction restoring agent of main component with the natural mineral, it is characterized in that, described surface-modifying agent is one or more the mixture in the following component:
Span60, Tween 60 or Span80.
7, according to claim 1 to 6 arbitrary described be the Antifriction restoring agent of main component with the natural mineral, it is characterized in that, be to be prepared from by the preparation method who may further comprise the steps:
I, each component is carried out proportioning according to described mass ratio;
II, raw material that proportioning in I step is good are after ball mill mixes, and homogenizing was handled 18~24 hours under 70~80 ℃ temperature, obtained the powder of 0.5~1.2 micron of mean particle size again through ball mill grinding.
8, as claim 1 to 7 arbitrary described be the preparation method of the Antifriction restoring agent of main component with the natural mineral, may further comprise the steps:
I, each component is carried out proportioning according to described mass ratio;
II, raw material that proportioning in I step is good are after ball mill mixes, and homogenizing was handled 18~24 hours under 70~80 ℃ temperature, obtained the powder of 0.5~1.2 micron of mean particle size again through ball mill grinding.
9, repair gel a kind of containing, contain: the described Antifriction restoring agent of 60~70 mass parts and the lubricating oil of 30~40 mass parts just like the antifriction of the arbitrary described Antifriction restoring agent of claim 1 to 7.
10, gel is repaired in antifriction according to claim 9, it is characterized in that, and be to be prepared from: the Antifriction restoring agent of described proportioning is mixed with lubricated oil phase, under 70~80 ℃ of temperature, stirred 2~3 hours by the method that may further comprise the steps.
11, repair lubricating grease a kind of containing, contain the described Antifriction restoring agent of phase blended 1~3 mass parts and the industrial grease of 97~99 mass parts just like the antifriction of the arbitrary described Antifriction restoring agent of claim 1 to 7.
12, repair lubricating oil a kind of containing, contain the Antifriction restoring agent of 0.5~2 mass parts and the industrial lubricant of 98~99.5 mass parts just like the antifriction of the arbitrary described Antifriction restoring agent of claim 1 to 7.
13, lubricating oil is repaired in antifriction according to claim 12, it is characterized in that, and be to be prepared from: the Antifriction restoring agent of above proportioning is mixed with the industrial lubrication oil phase, under 70~80 ℃ of temperature, stirred 2~3 hours by the method that may further comprise the steps.
CNB2005100929964A 2005-08-26 2005-08-26 Antifriction repairing agent with natural minerals as main components, preparation method and application Active CN100497514C (en)