Coal, the special-purpose anti-agar of ore dressing stone flour
Technical field:
The present invention relates to the anti-agar of a kind of special use, especially relate to a kind of anti-agar of special use that coal is antifreeze, the ore dressing stone flour is antifreeze that is mainly used in that is applicable to industries such as coal and ore dressing stone flour.
Background technology:
Present China train in the winter time transports in the process of coal or ore powder, because coal, ore powder itself and and the freezing of railway carriage, caused a lot of difficulties for traffic unit and user, cause many unnecessary financial losses, in order to address this problem, the coal of our research and development, ore special use prevent that agar is significant.
Summary of the invention:
The object of the present invention is to provide and a kind ofly be used for preventing coal, ore dressing stone flour itself is antifreeze or prevents the special-purpose anti-agar of a kind of coal, ore dressing stone flour that coal, ore dressing stone flour and railway carriage freeze in transportation.
Purpose of the present invention is implemented by following technical scheme: it includes: Calcium dichloride dihydrate (CaCL
22H
2O), inhibiter, rust inhibitor (Na
2NO
2), slipproofing agent (Na
2B
4O
710H
2O), adhesive agent (carboxymethyl cellulose) and ammoniacal liquor, by weight, described Calcium dichloride dihydrate (CaCL
22H
2O) content is 800~900 parts, and described inhibiter content is 30~100 parts, described rust inhibitor (Na
2NO
2) content is 10~35 parts, described slipproofing agent (Na
2B
4O
710H
2O) content is 10~20 parts, and described adhesive agent (carboxymethyl cellulose) content is 20~60 parts, then with above-mentioned composition after fusion, stirring, powder process, add ammoniacal liquor, make the pH value of above-mentioned composition 7~9, promptly make anti-agar.
By weight, described Calcium dichloride dihydrate (CaCL
22H
2O) content is preferably 800~900 parts; Inhibiter content is preferably 40~80 parts; Rust inhibitor (Na
2NO
2) content is preferably 28~32 parts; Slipproofing agent (Na
2B
4O
710H
2O) content is preferably 12~15 parts; Adhesive agent (carboxymethyl cellulose) content is preferably 25~30 parts.
Described inhibiter includes polymerization calcium wolframate, amino dodecane base polyphosphonic acid ammonium, calglucon, wooden calcium phosphate, by weight, described polymerization calcium wolframate content is that 35 parts~45 parts, amino dodecane base polyphosphonic acid ammonium content are that 25 parts~30 parts, gluconic acid calcium contents are that 15 parts~20 parts, wooden calcium phosphate content are 8~10 parts.This inhibiter is the high-efficient corrosion inhibitor of muriate salt and high chloride ion medium, can effectively suppress chlorion corrosion of metal is damaged, and slows down the destruction of chlorion to metal surface protection film and intergranular structure, the work-ing life of significant prolongation equipment.Inhibiter can prevent the corrosive damage that frostproofer causes the environment metallic facility in addition.Nontoxic non-corrosiveness, safe and harmless, pollution-free to environment for use.
Advantage of the present invention is: the water-absorbent of this product utilization calcium chloride is extremely strong, is exposed in the air very easily deliquescence, and is soluble in water, emits a large amount of heat simultaneously, and multiple auxiliary agent is made anti-agar in addition.Product has high-level efficiency, low freezing point, easily dissolving, low burn into advantage cheaply.This product antifreezing effect is strong, and suitable operating temperature range is big, reduces the loss of coal, ore powder in the transportation.And after powdered iron ore is antifreeze, when smelting, can effectively remove the sulphur in the iron.
Embodiment:
Embodiment 1: produce the anti-agar of 1000 grams and include: Calcium dichloride dihydrate (CaCL
22H
2O): 800 grams; Inhibiter: 100 grams, wherein inhibiter includes the polymerization calcium wolframate: 40 grams, amino dodecane base polyphosphonic acid ammonium: 35 grams, calglucon: 15 grams, wooden calcium phosphate: 10 grams; Rust inhibitor (Na
2NO
2): 35 grams; Slipproofing agent (Na
2B
4O
710H
2O): 20 grams; Adhesive agent (carboxymethyl cellulose): 45 grams; Through fusion, stirring, after mixing, making powdery, add ammoniacal liquor, make the pH value of above-mentioned composition 7~9, promptly make anti-agar.
Embodiment 2: produce the anti-agar of 1000 grams and include: Calcium dichloride dihydrate (CaCL
22H
2O): 820 grams; Inhibiter: 80 grams, wherein inhibiter includes the polymerization calcium wolframate: 40 grams, amino dodecane base polyphosphonic acid ammonium: 24 grams, calglucon: 16 grams, wooden calcium phosphate: 8 grams; Rust inhibitor (Na
2NO
2): 30 grams; Slipproofing agent (Na
2B
4O
710H
2O): 10 grams; Adhesive agent (carboxymethyl cellulose): 57 grams; Through fusion, stir, mix, make powdery after, add ammoniacal liquor, make the pH value of above-mentioned composition 7~9, promptly make anti-agar.
Embodiment 3: produce the anti-agar of 1000 grams and include: Calcium dichloride dihydrate (CaCL
22H
2O): 860 grams; Inhibiter: 50 grams, wherein inhibiter includes the polymerization calcium wolframate: 20 grams, amino dodecane base polyphosphonic acid ammonium: 18 grams, calglucon: 10 grams, wooden calcium phosphate: 5 grams; Rust inhibitor (Na
2NO
2): 20 grams; Slipproofing agent (Na
2B
4O
710H
2O): 15 grams; Adhesive agent (carboxymethyl cellulose): 55 grams; Through fusion, stir, mix, make powdery after, add ammoniacal liquor, make the pH value of above-mentioned composition 7~9, promptly make anti-agar.
Embodiment 4: produce the special-purpose anti-agar of 1000 grams and include: Calcium dichloride dihydrate (CaCL
22H
2O): 900 grams; Inhibiter: 40 grams, wherein inhibiter includes the polymerization calcium wolframate: 16 grams, amino dodecane base polyphosphonic acid ammonium: 12 grams, calglucon: 8 grams, wooden calcium phosphate: 4 grams; Rust inhibitor (Na
2NO
2): 10 grams; Slipproofing agent (Na
2B
1O
710H
2O): 10 grams; Adhesive agent (carboxymethyl cellulose): 40 grams; Through fusion, stir, mix, make powdery after, add ammoniacal liquor, make the pH value of above-mentioned composition 7~9, promptly make anti-agar.
Four above embodiment can be according to the water content of at that time temperature and coal or ore in concrete the use different, for different ratios solution, the ratio of Ru Shui and anti-agar is that solution such as 1: 0.4,1: 0.5,1: 0.8,1: 1.0,1: 1.2 is spread on the coal ore powder in order to avoid cause waste to water with its dilution.