CN1434086A - Interior wall coating and preparation method thereof - Google Patents

Interior wall coating and preparation method thereof Download PDF

Info

Publication number
CN1434086A
CN1434086A CN 03117396 CN03117396A CN1434086A CN 1434086 A CN1434086 A CN 1434086A CN 03117396 CN03117396 CN 03117396 CN 03117396 A CN03117396 A CN 03117396A CN 1434086 A CN1434086 A CN 1434086A
Authority
CN
China
Prior art keywords
ion
interior wall
distilled water
lime carbonate
coating
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
CN 03117396
Other languages
Chinese (zh)
Other versions
CN1210358C (en
Inventor
刘晓刚
肖惠文
刘肖莉
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Individual
Original Assignee
Individual
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Individual filed Critical Individual
Priority to CN 03117396 priority Critical patent/CN1210358C/en
Publication of CN1434086A publication Critical patent/CN1434086A/en
Application granted granted Critical
Publication of CN1210358C publication Critical patent/CN1210358C/en
Anticipated expiration legal-status Critical
Expired - Fee Related legal-status Critical Current

Abstract

The present invention relates to an interior wall coat and its preparation method. Said interior cost is composed of ground coat, middle coat and external coat, and is characterized by that every layer of said coat contains its respective raw material composition and is made up by adopting a certain preparation process. Said coat is no-toxic, has no abnormal smell, has no radioactivity, contains no harmful substances of formaldehyde, etc. and has the features of resisting fungus, resisting damp, resisting corrosion, resisting smoke and steam, no scaling and seasily cleaning, and is suitable for brush-coating interior wall of color preparation workshop, Chinese medicine extraction workshop, Chinese medicinal material storehouse and color and oil-containing workshop of food industry.

Description

A kind of interior wall coating and preparation method
Technical field
The present invention relates to a kind of coating, the interior wall coating that particularly a kind of pharmaceutical industry and food service industry are used.
Background technology
The interior wall coating of pharmaceutical industry and food service industry use at present adopts paint or emulsion paint mostly.Paint can discharge the organic solvent gas poisonous, that peculiar smell is arranged in the brushing process, and can be absorbed a part by metope, treat the paint film breakage after, slow release is come out, and environment is caused chronic pollution.Particularly, after shaggy Chinese medicinal materials adsorbs these smells, will influence the quality of medicinal material at pharmaceutical industry.Then because coating is too thin, it is stifling to be difficult to bear secular burn into for emulsion paint, chaps, comes off and lacquer painting takes place.Above-mentioned interior wall coating wall surface coated, be difficult to reach the health regulation requirement of country to pharmaceutical industry, food service industry production plant, particularly when envrionment conditions is abominable, coloured preparation workshop, traditional Chinese medicine extraction workshop, Chinese medicinal materials storehouse as pharmaceutical industry, the coloured food products workshop of food service industry, oleaginous food workshop etc., above-mentioned interior wall coating is powerless especially.
Summary of the invention
Technical problem to be solved by this invention, exactly at existing interior wall coating exist poisonous, peculiar smell, not corrosion-resistant, stifling, caducous shortcoming are arranged, provide a kind of nontoxic free from extraneous odour, corrosion-resistant, anti-stifling, can clean coloured contaminant, mildew-resistant, moistureproof adeciduate interior wall coating.
The technical scheme that the present invention solves its technical problem employing is: a kind of interior wall coating, and by priming paint, middle coating intermediate, outer layer coating is formed, and it is characterized in that: the described priming paint of a. is pressed column weight amount proportioning by following raw materials according and is formed:
Ion-exchange distilled water 80~95
Polyvinyl alcohol 7~12
Silicon sol 10~25
Sodium Benzoate 0.4~0.6
Lime carbonate 100~120
Calcium of intensifiens 15~25
Calcium hydroxide 12~28
Calcium hydroxide magnesium 6~12; B. described middle coating intermediate is pressed column weight amount proportioning by following raw materials according and is formed:
Ion-exchange distilled water 40~60
Titanium dioxide 6~15
Wilkinite 3~8
Wollastonite pure aluminium silicate 3~6
Lime carbonate 2~6
Sodium hexametaphosphate 99 0.5~1
Interpolymer latex of polystyrene and acrylic ester 40~60
Tributyl phosphate 0.2~0.4
Sodium Benzoate 1~2
Phenylcarbinol 1.5~3; C. described outer layer coating is pressed column weight amount proportioning by following raw materials according and is formed:
Ion-exchange distilled water 15~25
Titanium dioxide 3~5
Aerosil 0.1~0.25
Wilkinite 2~5
Lime carbonate 2~4
Interpolymer latex of polystyrene and acrylic ester 70~80
Tributyl phosphate 0.4~0.8
Water-based silicone oil 0.1~0.2
Parabens 0.05~0.1
Composite mildew inhibitor 1.5~3
Phenylcarbinol 2~5
Ethylene glycol 2~3.
The preparation method of interior wall coating of the present invention is: add raw material by above-mentioned weight proportion, press following prepared: a. priming paint preparation method:
(1) in ion-exchange distilled water, add polyvinyl alcohol, dash to polyvinyl alcohol with steam and dissolve fully,
(2) in (1), add Sodium Benzoate, treat its dissolving cooling after,
(3) in (2), add silicon sol, lime carbonate, Calcium of intensifiens, calcium hydroxide, calcium hydroxide magnesium successively, stir, form through grinding; B. middle coating intermediate preparation method:
(1) in ion-exchange distilled water, add Sodium Benzoate, titanium dioxide, wilkinite, wollastonite pure aluminium silicate, lime carbonate, Sodium hexametaphosphate 99, stir, grind,
(2) stirring adds interpolymer latex of polystyrene and acrylic ester, tributyl phosphate, phenylcarbinol down successively in (1), stirs, and forms through grinding; C. outer layer coating preparation method:
(1) in ion-exchange distilled water, add composite mildew inhibitor, aerosil, titanium dioxide, lime carbonate, wilkinite, stir, grind,
(2) stirring adds this ethylene-acrylate copolymer emulsion, tributyl phosphate, water-based silicone oil, phenylcarbinol, parabens, ethylene glycol down successively in (1), stirs, and grinding forms.
Above-mentioned interior wall coating is the interior wall coating that is used for coloured Drug Manufacturing Room.
The invention has the beneficial effects as follows: preparation technology is simple, the nontoxic free from extraneous odour of the interior wall coating of preparation, "dead", do not contain objectionable impuritiess such as formaldehyde.And have corrosion-resistant, anti-ly fumigate, do not come off, the characteristics of easy cleaning.Be particularly suitable for the interior wall brushing in coloured, the oil-containing workshop etc. of the coloured preparation of pharmaceutical industry workshop, traditional Chinese medicine extraction workshop, Chinese medicinal materials storehouse and food service industry.
Embodiment
Below in conjunction with embodiment, describe technical scheme of the present invention in detail.
Interior wall coating of the present invention is by priming paint, middle coating intermediate, and outer layer coating is formed, and it is characterized in that: the described priming paint of a. is pressed column weight amount proportioning by following raw materials according and is formed:
Ion-exchange distilled water 80~95
Polyvinyl alcohol 7~12
Silicon sol 10~25
Sodium Benzoate 0.4~0.6
Lime carbonate 100~120
Calcium of intensifiens 15~25
Calcium hydroxide 12~28
Calcium hydroxide magnesium 6~12; B. described middle coating intermediate is pressed column weight amount proportioning by following raw materials according and is formed:
Ion-exchange distilled water 40~60
Titanium dioxide 6~15
Wilkinite 3~8
Wollastonite pure aluminium silicate 3~6
Lime carbonate 2~6
Sodium hexametaphosphate 99 0.5~1
Interpolymer latex of polystyrene and acrylic ester 40~60
Tributyl phosphate 0.2~0.4
Sodium Benzoate 1~2
Phenylcarbinol 1.5~3; C. described outer layer coating is pressed column weight amount proportioning by following raw materials according and is formed:
Ion-exchange distilled water 15~25
Titanium dioxide 3~5
Aerosil 0.1~0.25
Wilkinite 2~5
Lime carbonate 2~4
Interpolymer latex of polystyrene and acrylic ester 70~80
Tributyl phosphate 0.4~0.8
Water-based silicone oil 0.1~0.2
Parabens 0.05~0.1
Composite mildew inhibitor 1.5~3
Phenylcarbinol 2~5
Ethylene glycol 2~3.
Embodiment: a. priming paint preparation method:
(1) in 85kg ion-exchange distilled water, add the 8kg polyvinyl alcohol, dash to polyvinyl alcohol with steam and dissolve fully,
(2) in (1), add the 0.5kg Sodium Benzoate, treat its dissolving cooling after,
(3) in (2), add 18kg silicon sol, 110kg lime carbonate, 18kg Calcium of intensifiens, 16kg calcium hydroxide, 10kg calcium hydroxide magnesium successively, stir,
Form through grinding; B. middle coating intermediate preparation method:
(1) in 50kg ion-exchange distilled water, add 1.5kg Sodium Benzoate, 10kg titanium dioxide, 5kg wilkinite, 3kg wollastonite pure aluminium silicate, 4kg lime carbonate, 0.5kg Sodium hexametaphosphate 99, stir, grind,
(2) stirring adds 50kg interpolymer latex of polystyrene and acrylic ester, 0.3kg tributyl phosphate, 1.5kg phenylcarbinol down successively in (1), stirs, and forms through grinding; C. outer layer coating preparation method:
(1) in 15kg ion-exchange distilled water, add 2kg composite mildew inhibitor, 0.15kg aerosil, 4kg titanium dioxide, 3kg lime carbonate, 4kg wilkinite, stir, grind,
(2) stirring adds this ethylene-acrylate of 75kg copolymer emulsion, 0.5kg tributyl phosphate, 0.15kg water-based silicone oil, 4kg phenylcarbinol, 0.06kg parabens, 2.5kg ethylene glycol down successively in (1), stirs, and grinding forms.
Above-mentioned interior wall coating is the interior wall coating that is used for coloured Drug Manufacturing Room.
Interior wall coating constructional method of the present invention is that metope is used earlier the priming paint brushing after conventional clean, require no scratch, no drip, wait to parch back brushing middle coating intermediate, after middle coating intermediate parches, with behind No. 200 waterproof abrasive paper sand millings, remove sand and dust and be coated with and brush outer layer coating and get final product.Adopt above-mentioned interior wall coating wall surface coated, nontoxic free from extraneous odour, "dead", do not contain objectionable impurities such as formaldehyde, and mildew-resistant, protection against the tide, corrosion-resistant, anti-ly fumigate, do not come off, easy cleaning.Be particularly suitable for the interior wall brushing in coloured, the oil-containing workshop etc. of the coloured preparation of pharmaceutical industry workshop, traditional Chinese medicine extraction workshop, Chinese medicinal materials storehouse and food service industry.

Claims (4)

1. interior wall coating, by priming paint, middle coating intermediate, outer layer coating is formed, and it is characterized in that: the described priming paint of a. is pressed column weight amount proportioning by following raw materials according and is formed:
Ion-exchange distilled water 80~95
Polyvinyl alcohol 7~12
Silicon sol 10~25
Sodium Benzoate 0.4~0.6
Lime carbonate 100~120
Calcium of intensifiens 15~25
Calcium hydroxide 12~28
Calcium hydroxide magnesium 6~12; B. described middle coating intermediate is pressed column weight amount proportioning by following raw materials according and is formed:
Ion-exchange distilled water 40~60
Titanium dioxide 6~15
Wilkinite 3~8
Wollastonite pure aluminium silicate 3~6
Lime carbonate 2~6
Sodium hexametaphosphate 99 0.5~1
Interpolymer latex of polystyrene and acrylic ester 40~60
Tributyl phosphate 0.2~0.4
Sodium Benzoate 1~2
Phenylcarbinol 1.5~3; C. described outer layer coating is pressed column weight amount proportioning by following raw materials according and is formed:
Ion-exchange distilled water 15~25
Titanium dioxide 3~5
Aerosil 0.1~0.25
Wilkinite 2~5
Lime carbonate 2~4
Interpolymer latex of polystyrene and acrylic ester 70~80
Tributyl phosphate 0.4~0.8
Water-based silicone oil 0.1~0.2
Parabens 0.05~0.1
Composite mildew inhibitor 1.5~3
Phenylcarbinol 2~5
Ethylene glycol 2~3.
2. interior wall coating as claimed in claim 1 is characterized in that: the described priming paint of a. is pressed column weight amount proportioning by following raw materials according and is formed:
Ion-exchange distilled water 85
Polyvinyl alcohol 8
Silicon sol 18
Sodium Benzoate 0.5
Lime carbonate 110
Calcium of intensifiens 18
Calcium hydroxide 16
Calcium hydroxide magnesium 10; B. described middle coating intermediate is pressed column weight amount proportioning by following raw materials according and is formed:
Ion-exchange distilled water 50
Titanium dioxide 10
Wilkinite 5
Wollastonite pure aluminium silicate 3
Lime carbonate 4
Sodium hexametaphosphate 99 0.5
Interpolymer latex of polystyrene and acrylic ester 50
Tributyl phosphate 0.3
Sodium Benzoate 1.5
Phenylcarbinol 1.5; C. described outer layer coating is pressed column weight amount proportioning by following raw materials according and is formed:
Ion-exchange distilled water 15
Titanium dioxide 4
Aerosil 0.15
Wilkinite 4
Lime carbonate 3
Interpolymer latex of polystyrene and acrylic ester 75
Tributyl phosphate 0.5
Water-based silicone oil 0.15
Parabens 0.06
Composite mildew inhibitor 2
Phenylcarbinol 4
Ethylene glycol 2.5.
3. interior wall coating as claimed in claim 1 is characterized in that: add raw material by above-mentioned weight proportion, press following prepared: a. priming paint compound method:
(1) in ion-exchange distilled water, add polyvinyl alcohol, dash to polyvinyl alcohol with steam and dissolve fully,
(2) in (1), add Sodium Benzoate, treat its dissolving cooling after,
(3) in (2), add silicon sol, lime carbonate, Calcium of intensifiens, calcium hydroxide, calcium hydroxide magnesium successively, stir, form through grinding; B. middle coating intermediate compound method:
(1) in ion-exchange distilled water, add Sodium Benzoate, titanium dioxide, wilkinite, wollastonite pure aluminium silicate, lime carbonate, Sodium hexametaphosphate 99, stir, grind,
(2) stirring adds interpolymer latex of polystyrene and acrylic ester, tributyl phosphate, phenylcarbinol down successively in (1), stirs, and forms through grinding; C. outer layer coating compound method:
(1) in ion-exchange distilled water, add composite mildew inhibitor, aerosil, titanium dioxide, lime carbonate, wilkinite, stir, grind,
(2) stirring adds this ethylene-acrylate copolymer emulsion, tributyl phosphate, water-based silicone oil, phenylcarbinol, parabens, ethylene glycol down successively in (1), stirs, and grinding forms.
4. interior wall coating as claimed in claim 1 is characterized in that: described interior wall coating is the interior wall coating that is used for coloured Drug Manufacturing Room.
CN 03117396 2003-03-04 2003-03-04 Interior wall coating and preparation method thereof Expired - Fee Related CN1210358C (en)