CN121850737A - Method for improving bonding force of inorganic thermal control coating on surface of carbon/carbon composite material - Google Patents

Method for improving bonding force of inorganic thermal control coating on surface of carbon/carbon composite material

Info

Publication number
CN121850737A
CN121850737A CN202511693380.6A CN202511693380A CN121850737A CN 121850737 A CN121850737 A CN 121850737A CN 202511693380 A CN202511693380 A CN 202511693380A CN 121850737 A CN121850737 A CN 121850737A
Authority
CN
China
Prior art keywords
carbon
composite material
thermal control
control coating
carbon composite
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CN202511693380.6A
Other languages
Chinese (zh)
Inventor
任超龙
靳宇
白晶莹
张家强
张立功
李思振
王兵存
周华珍
孟腾
董理
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Beijing Satellite Manufacturing Factory Co Ltd
Original Assignee
Beijing Satellite Manufacturing Factory Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Beijing Satellite Manufacturing Factory Co Ltd filed Critical Beijing Satellite Manufacturing Factory Co Ltd
Priority to CN202511693380.6A priority Critical patent/CN121850737A/en
Publication of CN121850737A publication Critical patent/CN121850737A/en
Pending legal-status Critical Current

Abstract

本发明提供了一种提升碳/碳复合材料表面无机热控涂层结合力的方法,包括:将碳/碳复合材料置于无水乙醇中,超声清洗,干燥,完成超声清洗;采用激光在碳/碳复合材料表面连续扫描,完成激光清洗;将表面处理剂喷涂在激光清洗后的碳/碳复合材料表面;将无机热控涂料喷涂在已喷涂表面处理剂的碳/碳复合材料表面,阴干,固化,在碳/碳复合材料表面成型无机热控涂层。本发明方法通过超声清洗、激光清洗、表面处理剂桥连作用,提高了碳/碳复合材料表面无机热控涂层的结合力。

This invention provides a method for improving the adhesion of an inorganic thermal control coating on the surface of carbon/carbon composite materials, comprising: placing the carbon/carbon composite material in anhydrous ethanol, ultrasonically cleaning, and drying to complete the ultrasonic cleaning; continuously scanning the surface of the carbon/carbon composite material with a laser to complete laser cleaning; spraying a surface treatment agent onto the laser-cleaned surface of the carbon/carbon composite material; spraying an inorganic thermal control coating onto the surface of the carbon/carbon composite material with the surface treatment agent, air-drying, and curing to form an inorganic thermal control coating on the surface of the carbon/carbon composite material. This invention improves the adhesion of the inorganic thermal control coating on the surface of the carbon/carbon composite material through the bridging effect of ultrasonic cleaning, laser cleaning, and the surface treatment agent.

Description

Method for improving bonding force of inorganic thermal control coating on surface of carbon/carbon composite material
Technical Field
The invention belongs to the technical field of improving the binding force between a coating and a base material, and particularly relates to a method for improving the binding force of an inorganic thermal control coating on the surface of a carbon/carbon composite material.
Background
The carbon/carbon composite material (hereinafter referred to as C/C composite material) is a carbon fiber reinforced ultra-high temperature ceramic matrix composite material, and has good high temperature strength, high temperature fracture toughness, excellent thermal shock resistance, oxidation resistance, ablation resistance and reliability. In recent years, with the increase of the demand of the aerospace field for light-weight high-strength materials, the application of C/C composite materials on spacecrafts is increasing. For example, the traditional spacecraft thermal control system often adopts metal materials such as copper, and the like, and has the problems of large area density, low modulus, easy deformation, insufficient strength, low heat transfer efficiency under high-power heat flow and the like, so that the future application requirements are difficult to meet. The high heat conduction C/C composite material has the excellent characteristics of light weight, high temperature resistance, gao Bijiang, high-modulus, stable physical and chemical properties and the like, and becomes the preferred material for preparing the light-weight high-efficiency radiator. However, the C/C composite material is black, so that solar absorption is high, and radiation and heat dissipation capabilities of the C/C composite material are severely restricted. Therefore, a layer of high-temperature-resistant low-absorption high-emissivity thermal control coating is required to be prepared on the surface of the spacecraft thermal control coating so as to adjust the thermal and optical properties of the spacecraft and further realize the thermal control effect.
The thermal control coating is divided into an organic coating and an inorganic coating, and the common high-temperature-resistant low-absorption high-emissivity thermal control coating at present is generally an inorganic coating, such as a multi-element doped titanium oxide coating. However, the C/C composite material is a lipophilic and hydrophobic material, and the aqueous inorganic coating is difficult to wet and spread on the surface of the C/C composite material, so that the bonding force of the coating is greatly challenged. Therefore, it is necessary to develop a new surface treatment method for the C/C composite material to enhance the bonding force of the inorganic coating on the surface of the C/C composite material.
Disclosure of Invention
In order to overcome the defects in the prior art, the inventor performs intensive research, provides a method for improving the bonding force of the inorganic thermal control coating on the surface of the carbon/carbon composite material, and solves the problem that the bonding force of the inorganic thermal control coating on the surface of the carbon/carbon composite material is poor.
The technical scheme provided by the invention is as follows:
A method for improving the bonding force of an inorganic thermal control coating on the surface of a carbon/carbon composite material, comprising the following steps:
Placing the carbon/carbon composite material in absolute ethyl alcohol, carrying out ultrasonic cleaning, and drying to complete ultrasonic cleaning;
Laser is adopted to continuously scan the surface of the carbon/carbon composite material, so as to finish laser cleaning;
Spraying a surface treating agent on the surface of the carbon/carbon composite material subjected to laser cleaning;
spraying the inorganic thermal control coating on the surface of the carbon/carbon composite material sprayed with the surface treating agent, drying in the shade, solidifying and forming the inorganic thermal control coating on the surface of the carbon/carbon composite material.
The method for improving the bonding force of the inorganic thermal control coating on the surface of the carbon/carbon composite material has the following beneficial effects:
(1) Aiming at the problems that the C/C composite material has larger brittleness and is easy to damage materials in the conventional pretreatment modes such as manual polishing, sand blasting and the like, the invention adopts the laser cleaning for pretreatment, thereby effectively avoiding the damage risk of manual operation on the materials;
(2) The invention adopts heat-resistant silane coupling agent solution as surface treating agent, on one hand, the silane coupling agent is an organic silicon compound with special structure, the two ends of the molecule of the silane coupling agent respectively contain groups which can react with inorganic materials and organic materials, and a 'molecular bridge' is formed at the interface of the two through compound bonding, thereby effectively enhancing the bonding force of inorganic coating on the surface of C/C composite material;
(3) The invention selects the multielement doped titanium oxide as the active ingredient of the thermal control coating, utilizes the trivalent oxide to dope the titanium oxide, introduces oxygen vacancies while generating lattice distortion, reduces lattice symmetry, improves carrier concentration, widens infrared absorption band, obtains high emissivity while keeping low solar absorption ratio, realizes spectrum selective absorption, has 600 ℃ infrared emissivity of 0.80-0.85 and solar absorption ratio of 0.20-0.35, and has excellent high-temperature radiating effect.
Drawings
FIG. 1 is a graph showing the wettability of deionized water on the surface of a carbon/carbon composite material before and after laser cleaning;
FIG. 2 is a cross-sectional view of the coating prepared in example 1;
FIG. 3 is a cross-sectional view of the coating prepared in comparative example 1;
FIG. 4 is a cross-sectional view of the coating prepared in comparative example 2;
fig. 5 is a cross-sectional result of the coating prepared in comparative example 3.
Detailed Description
The features and advantages of the present invention will become more apparent and clear from the following detailed description of the invention.
The word "exemplary" is used herein to mean "serving as an example, embodiment, or illustration. Any embodiment described herein as "exemplary" is not necessarily to be construed as preferred or advantageous over other embodiments.
The invention provides a method for improving the bonding force of an inorganic thermal control coating on the surface of a carbon/carbon composite material, which comprises the following steps:
(1) And (3) ultrasonic cleaning, namely placing the C/C composite material in absolute ethyl alcohol, performing ultrasonic vibration for 1-2 hours, then drying by compressed air, and standing for 1-2 hours.
(2) And (3) laser cleaning, namely, applying laser to the surface of the C/C composite material to enable the light beam to continuously sweep the surface of the C/C composite material for 2-3 times.
In the step, the laser wavelength is less than 400nm (ultraviolet laser), for example 355nm, the average output power of the laser is 500-2000W, the laser pulse frequency is 10-100 kHz, the laser output pulse width is 10-50 ns, and the laser scanning speed is 5-50 mm/s.
The ultraviolet band laser is selected for laser cleaning, on one hand, the ultraviolet laser has the characteristic of cold working or cold ablation, heat is not diffused during scanning cleaning, oxidation damage or deformation of the C/C composite material due to local overtemperature is not caused, on the other hand, the ultraviolet photon energy is high, chemical bonds of organic materials can be directly broken, the organic materials are not melted and gasified by means of heat, broken chemical bonds have certain activity, chemical bonds can be generated with a surface treating agent, and the binding force of a coating is effectively improved.
(3) And (3) spraying a surface treating agent, namely spraying the surface treating agent on the surface of the C/C composite material treated in the step (2) for 2-3 times by adopting an air spraying method.
In the step, the surface treating agent comprises the following components in parts by mass:
100 parts of a silane coupling agent;
50-200 parts of absolute ethyl alcohol;
10-100 parts of deionized water.
Wherein the silane coupling agent is a heat-resistant silane coupling agent and is selected from at least one of Y-5475 or Y-5669.
(4) And (3) preparing a thermal control coating, namely spraying an inorganic thermal control coating on the surface of the C/C composite material treated in the step (3) by adopting an air spraying method.
In the step, the inorganic thermal control coating comprises the following components in parts by mass:
100 parts of thermal control filler;
50-200 parts of an inorganic binder;
100-300 parts of deionized water.
The inorganic binder is at least one of silicate binder or phosphate binder, such as potassium silicate or potassium phosphate.
The chemical composition of the thermal control filler is Ti 1-xMxO2-0.5x, M represents one or more of Gd, yb and Ga, x is more than 0 and less than or equal to 0.5, and the thermal control filler is called multi-element doped titanium oxide.
Preferably, the chemical composition of the thermal control filler is Ti 1-xGdxO2-0.5x, 0< x≤0.5. Or the chemical composition of the thermal control filler is Ti 1-xYbxO2-0.5x, wherein x is more than 0 and less than or equal to 0.5. Or the chemical composition of the thermal control filler is Ti 1-xGaxO2-0.5x, wherein x is more than 0 and less than or equal to 0.5. Or the chemical composition of the thermal control filler is Ti 1-x(GdyYb1-y)xO2-0.5x, wherein x is 0< 0.5, y is 0< 1. Or the chemical composition of the thermal control filler is Ti 1-x(GdyGa1-y)xO2-0.5x, wherein x is 0< 0.5, y is 0< 1. Or the chemical composition of the thermal control filler is Ti 1-x(YbyGa1-y)xO2-0.5x, wherein x is 0< 0.5, y is 0< 1. Or the chemical composition of the thermal control filler is as follows Ti1-x(GdyYbzGak)xO2-0.5x,0<x≤0.5,0<y<1,0<z<1,0<k<1,y+z+k=1.
The preparation method of the thermal control filler comprises the following steps:
And (4.1) weighing the dried titanium dioxide and trivalent oxide powder according to a stoichiometric ratio, adding the mixture into a ball milling tank, taking deionized water as a ball milling medium, taking zirconia balls as grinding balls, and ball milling and mixing for 8-12 hours at 300-500 r/min. Wherein the trivalent oxide powder is one or more of gadolinium oxide (Gd 2O3), ytterbium oxide (Yb 2O3) and gallium oxide (Ga 2O3) powder.
And (4.2) drying the ball-milled slurry for 12-24 hours at the temperature of 90-120 ℃.
And (4.3) sieving the dried powder into small-particle powder with uniform particle size by using a standard sieve with 100-400 meshes.
And (4.4) placing the sieved powder into an alumina crucible, placing the alumina crucible into a high-temperature furnace for solid phase synthesis, heating to 1300-1600 ℃ at a heating rate of 1-3 ℃ per minute, preserving heat for 12-24 h, and then cooling along with the furnace.
And (4.5) grinding the powder subjected to solid phase synthesis by using a mortar until the particle size is smaller than 1-3 mm, adding the powder into a ball milling tank, taking deionized water as a ball milling medium, taking zirconia balls as grinding balls, and performing ball milling and crushing for 12-24 hours at 300-500 r/min to ensure that the particle size of the powder subjected to ball milling is 1-5 mu m.
And (4.6) drying the slurry subjected to ball milling and crushing at 90-120 ℃ for 12-24 hours.
And (4.7) sieving the dried powder with a 100-400-mesh standard sieve to obtain small-particle powder with uniform particle size, thereby obtaining the thermal control filler.
The trivalent oxide is used for doping titanium dioxide, and generating an introduced oxygen vacancy while generating lattice distortion, so that the lattice symmetry is reduced, the carrier concentration is improved, the infrared absorption band is widened, the high emissivity is obtained, the low solar absorption ratio is kept, the spectrum selective absorption is realized, the infrared emissivity at 600 ℃ can reach 0.80-0.85, the solar absorption ratio is 0.20-0.35, the excellent high-temperature heat dissipation effect is realized, and the problems that the solar absorption of the traditional high-emissivity coating is relatively high and the heat dissipation capability of the coating is deteriorated are solved.
In the step, the environment temperature is 20-30 ℃ when the inorganic thermal control coating is sprayed by air, the environment relative humidity is 30-70%, and the thickness of the coating is 50-200 mu m.
(5) And (3) curing the coating, namely placing the inorganic thermal control coating in an environment with the temperature of 20-30 ℃ and the relative humidity of 40% -70%, drying in the shade for 12-24 hours, and then placing the inorganic thermal control coating in an oven with the temperature of 80-250 ℃ and drying for 4-12 hours.
Examples
Example 1
A forming method of an inorganic thermal control coating on the surface of a carbon/carbon composite material comprises the following steps:
(1) Placing the C/C composite material in absolute ethyl alcohol, ultrasonically vibrating for 2 hours, then drying by compressed air, and standing for 2 hours;
(2) Selecting an ultraviolet laser cleaning device with 355nm output wavelength, wherein the average output power is 1000W, the laser pulse frequency is 50kHz, the laser output pulse width is 10ns, the laser scanning speed is 10mm/s, and the laser spots act on the surface of the C/C composite material and continuously sweep for 3 times;
(3) Taking 100g of heat-resistant silane coupling agent Y-5475 g, adding 50g of absolute ethyl alcohol and 20g of deionized water, mixing and uniformly stirring to prepare a surface treating agent, and then spraying the surface treating agent on the surface of the C/C composite material treated in the step (2) for 2 times by adopting an air spraying method;
(4) Mixing 50g of Ti 0.5Gd0.5O1.75 powder (solar absorption ratio 0.30,600 ℃ emissivity 0.81), 50g of potassium silicate solution and 90g of deionized water uniformly by adopting a ball milling method to prepare a coating of an inorganic thermal control coating, and then spraying the coating on the surface of the C/C composite material treated in the step (3) by adopting an air spraying method;
(5) After the spraying is finished, the coating is placed in an environment with the temperature of 25-30 ℃ and the relative humidity of 40% -45% for drying in the shade for 15h, and then the coating is placed in a baking oven with the temperature of 200 ℃ for drying for 10h, so that the inorganic coating well combined with the C/C composite material is obtained.
As shown in figure 1, after laser cleaning, the wettability of deionized water on the surface of the C/C composite material is obviously increased, and the water-based inorganic coating is extremely easy to spread, which indicates that the surface of the C/C composite material after laser cleaning has good film forming property, and is favorable for improving the binding force of the coating. As shown in FIG. 2, after the surface of the C/C composite material is subjected to laser cleaning and spraying of the surface treatment agent, the surface of the coating prepared in the embodiment 1 is good in state, smooth and flat, and free of defects such as cracking and protruding, and the cross-cut result shows that the bonding force of the coating can reach the level 1.
Examples 2 to 7
A forming method of an inorganic thermal control coating on the surface of a carbon/carbon composite material comprises the following steps:
(1) Placing the C/C composite material in absolute ethyl alcohol, ultrasonically vibrating for 2 hours, then drying by compressed air, and standing for 2 hours;
(2) Selecting an ultraviolet laser cleaning device with 355nm output wavelength, wherein the average output power is 1000W, the laser pulse frequency is 50kHz, the laser output pulse width is 10ns, the laser scanning speed is 10mm/s, and the laser spots act on the surface of the C/C composite material and continuously sweep for 3 times;
(3) Taking 100g of heat-resistant silane coupling agent Y-5475 g, adding 50g of absolute ethyl alcohol and 20g of deionized water, mixing and uniformly stirring to prepare a surface treating agent, and then spraying the surface treating agent on the surface of the C/C composite material treated in the step (2) for 2 times by adopting an air spraying method;
(4) Taking 50g of heat control filler powder, 50g of potassium silicate solution and 90g of deionized water, uniformly mixing the materials by a ball milling method to prepare a coating of an inorganic heat control coating, and then spraying the coating on the surface of the C/C composite material treated in the step (3) by an air spraying method, wherein the heat control filler powder is selected from Ti 0.5Ga0.5O1.75 powder (solar absorption ratio 0.20,600 ℃ emissivity 0.80), ti 0.5Yb0.5O1.75 powder (solar absorption ratio 0.35,600 ℃ emissivity 0.82), ti 0.5(Gd0.5Yb0.5)0.5O1.75 powder (solar absorption ratio 0.31,600 ℃ emissivity 0.82), ti 0.5(Gd0.5Ga0.5)0.5O1.75 powder (solar absorption ratio 0.28,600 ℃ emissivity 0.82), ti 0.5(Yb0.5Ga0.5)0.5O1.75 powder (solar absorption ratio 0.33,600 ℃ emissivity 0.83) and Ti 0.5(Gd0.3Yb0.3Ga0.4)0.5O1.75 powder (solar absorption ratio 0.32,600 ℃ emissivity 0.84), and the heat control filler is prepared according to the preparation method;
(5) After the spraying is finished, the coating is placed in an environment with the temperature of 25-30 ℃ and the relative humidity of 40% -45% for drying in the shade for 15h, and then the coating is placed in a baking oven with the temperature of 200 ℃ for drying for 10h, so that the inorganic coating well combined with the C/C composite material is obtained.
After the surface of the C/C composite material is subjected to laser cleaning and spraying of a surface treatment agent, the surface state of the coating prepared in the examples 2-7 is good, smooth and flat, and the coating has no defects of cracking, protruding and the like, and the cross-cut result shows that the coating binding force can reach level 1.
Comparative example
Comparative example 1
A forming method of an inorganic thermal control coating on the surface of a carbon/carbon composite material comprises the following steps:
(1) Placing the C/C composite material in absolute ethyl alcohol, ultrasonically vibrating for 2 hours, then drying by compressed air, and standing for 2 hours;
(2) Mixing 50g of Ti 0.5Gd0.5O1.75 powder, 50g of potassium silicate solution and 90g of deionized water uniformly by adopting a ball milling method to prepare a coating of an inorganic thermal control coating, and then spraying the coating on the surface of the C/C composite material by adopting an air spraying method;
(3) After the spraying is finished, the coating is placed in an environment with the temperature of 25-30 ℃ and the relative humidity of 40-45% for drying in the shade for 15 hours, and then the coating is placed in a baking oven with the temperature of 200 ℃ for drying for 10 hours, so that the inorganic coating with extremely poor combination with the C/C composite material is obtained.
FIG. 3 shows the surface morphology of the inorganic coating prepared on the C/C composite material which is not subjected to laser cleaning and is not sprayed with the surface treatment agent in comparative example 1, the chapped coating surface can be seen, the morphology of the test piece edge and the internal coating is inconsistent, the edge has the current situation of bulge cracking, the coating is unevenly spread, and the cross-cut result shows that the coating binding force is extremely poor.
Comparative example 2
A forming method of an inorganic thermal control coating on the surface of a carbon/carbon composite material comprises the following steps:
(1) Placing the C/C composite material in absolute ethyl alcohol, ultrasonically vibrating for 2 hours, then drying by compressed air, and standing for 2 hours;
(2) Setting the output wavelength of the laser cleaning equipment to 532nm, the average output power to 1000W, the laser pulse frequency to 50kHz, the laser output pulse width to 10ns and the laser scanning speed to 10mm/s, so that a laser spot acts on the surface of the C/C composite material and continuously sweeps for 3 times;
(3) Uniformly mixing 50g of Ti 0.5Gd0.5O1.75 powder, 50g of potassium silicate solution and 90g of deionized water by adopting a ball milling method to prepare a coating of an inorganic thermal control coating, and then spraying the coating on the surface of the C/C composite material treated in the step (2) by adopting an air spraying method;
(4) After the spraying is finished, the coating is placed in an environment with the temperature of 25-30 ℃ and the relative humidity of 40-45% for drying in the shade for 15 hours, and then the coating is placed in a baking oven with the temperature of 200 ℃ for drying for 10 hours, so that the inorganic coating which is well combined with the C/C composite material is obtained.
Fig. 4 shows the surface morphology of the inorganic coating prepared in comparative example 2 on the C/C composite material which was laser cleaned but not sprayed with the surface treatment agent, and it can be seen that the coating showed flatness and smoothness, indicating that the inorganic coating was well spread, uniformly formed into a film, and the cross-hatch result showed a significant improvement in the coating binding force as compared with comparative example 1, but lower than the coating prepared in example 1.
Comparative example 3
A forming method of an inorganic thermal control coating on the surface of a carbon/carbon composite material comprises the following steps:
(1) Placing the C/C composite material in absolute ethyl alcohol, ultrasonically vibrating for 2 hours, then drying by compressed air, and standing for 2 hours;
(2) Taking 100g of heat-resistant silane coupling agent Y-5475 g, adding 50g of absolute ethyl alcohol and 20g of deionized water, mixing and uniformly stirring to prepare a surface treating agent, and then spraying the surface treating agent on the surface of the C/C composite material treated in the step (1) for 2 times by adopting an air spraying method;
(3) Uniformly mixing 50g of Ti 0.5Gd0.5O1.75 powder, 50g of potassium silicate solution and 90g of deionized water by adopting a ball milling method to prepare a coating of an inorganic thermal control coating, and then spraying the coating on the surface of the C/C composite material treated in the step (3) by adopting an air spraying method;
(4) After the spraying is finished, the coating is placed in an environment with the temperature of 25-30 ℃ and the relative humidity of 40-45% for drying in the shade for 15 hours, and then the coating is placed in a baking oven with the temperature of 200 ℃ for drying for 10 hours, so that the inorganic coating which is well combined with the C/C composite material is obtained.
Fig. 5 shows the surface morphology of the inorganic coating prepared on the C/C composite material which is not subjected to laser cleaning but sprayed with the surface treatment agent in comparative example 3, and although the cross-cut result shows that the coating has good bonding force with the C/C composite material, the surface state of the coating is poor, more small bulges exist, because the wettability of the inorganic coating on the surface of the C/C composite material which is not subjected to laser cleaning is poor, the coating is easy to aggregate to form small liquid drops after spraying, and the liquid drops solidify to form bulges after drying.
It can be seen from the combination of example 1 and comparative examples 1-3 that the laser cleaning and spray surface treatment agent can be combined in different aspects to improve the binding force of the inorganic coating on the surface of the C/C composite material.
The invention has been described in detail in connection with the specific embodiments and exemplary examples thereof, but such description is not to be construed as limiting the invention. It will be understood by those skilled in the art that various equivalent substitutions, modifications or improvements may be made to the technical solution of the present invention and its embodiments without departing from the spirit and scope of the present invention, and these fall within the scope of the present invention. The scope of the invention is defined by the appended claims.
What is not described in detail in the present specification is a well known technology to those skilled in the art.

Claims (10)

1. The method for improving the bonding force of the inorganic thermal control coating on the surface of the carbon/carbon composite material is characterized by comprising the following steps:
Placing the carbon/carbon composite material in absolute ethyl alcohol, carrying out ultrasonic cleaning, and drying to complete ultrasonic cleaning;
Laser is adopted to continuously scan the surface of the carbon/carbon composite material, so as to finish laser cleaning;
Spraying a surface treating agent on the surface of the carbon/carbon composite material subjected to laser cleaning;
spraying the inorganic thermal control coating on the surface of the carbon/carbon composite material sprayed with the surface treating agent, drying in the shade, solidifying and forming the inorganic thermal control coating on the surface of the carbon/carbon composite material.
2. The method for improving the bonding force of an inorganic thermal control coating on the surface of a carbon/carbon composite material according to claim 1, wherein in the step of laser cleaning, the laser wavelength is <400nm, the average output power of laser is 500-2000W, the pulse frequency of laser is 10-100 kHz, the pulse width of laser output is 10-50 ns, and the scanning speed of laser is 5-50 mm/s.
3. The method for improving the bonding force of an inorganic thermal control coating on the surface of a carbon/carbon composite material according to claim 1, wherein the surface treating agent comprises the following components in parts by mass:
100 parts of a silane coupling agent;
50-200 parts of absolute ethyl alcohol;
10-100 parts of deionized water.
4. The method for improving the bonding force of an inorganic thermal control coating on the surface of a carbon/carbon composite material according to claim 3, wherein the silane coupling agent is a heat-resistant silane coupling agent selected from at least one of Y-5475 or Y-5669.
5. The method for improving the bonding force of the inorganic thermal control coating on the surface of the carbon/carbon composite material according to claim 1, wherein the surface treatment agent is sprayed on the surface of the carbon/carbon composite material for 2-3 times.
6. The method for improving the bonding force of the inorganic thermal control coating on the surface of the carbon/carbon composite material according to claim 1, wherein the inorganic thermal control coating comprises the following components in parts by mass:
100 parts of thermal control filler;
50-200 parts of an inorganic binder;
100-300 parts of deionized water;
The chemical composition of the thermal control filler is Ti 1-xMxO2-0.5x, M represents one or more of Gd, yb and Ga, and x is more than 0 and less than or equal to 0.5.
7. The method for improving the bonding force of an inorganic thermal control coating on the surface of a carbon/carbon composite material according to claim 6, wherein the preparation method of the thermal control filler comprises the following steps:
Weighing dry titanium dioxide and trivalent oxide powder according to a stoichiometric ratio, wherein the trivalent oxide powder is one or more of gadolinium oxide, ytterbium oxide and gallium oxide powder;
Adding titanium dioxide and trivalent oxide powder into a ball milling tank, drying slurry after ball milling, and sieving the dried powder to obtain powder with uniform particle size;
solid phase synthesis is carried out on the sieved powder in a high-temperature environment, and after heat preservation, the powder is cooled along with a furnace;
and grinding and ball milling the powder after solid phase synthesis, drying slurry after ball milling, and sieving the dried powder to obtain the spectrum selective absorption heat control filler.
8. The method of claim 6, wherein the inorganic binder is at least one of a silicate binder or a phosphate binder.
9. The method for improving the bonding force of the inorganic thermal control coating on the surface of the carbon/carbon composite material according to claim 6, wherein the environmental temperature is 20-30 ℃ when the inorganic thermal control coating is sprayed, the environmental relative humidity is 30% -70%, and the thickness of the inorganic thermal control coating is preferably 50-200 μm.
10. The method for improving the bonding force of the inorganic thermal control coating on the surface of the carbon/carbon composite material according to claim 1, wherein the step of spraying the inorganic thermal control coating on the surface of the carbon/carbon composite material sprayed with the surface treatment agent, drying in the shade and solidifying comprises the steps of placing the inorganic thermal control coating in an environment with the temperature of 20-30 ℃ and the relative humidity of 40% -70% for 12-24 hours, placing the inorganic thermal control coating in an oven with the temperature of 80-250 ℃ and drying for 4-12 hours.
CN202511693380.6A 2025-11-18 2025-11-18 Method for improving bonding force of inorganic thermal control coating on surface of carbon/carbon composite material Pending CN121850737A (en)