10.9-Grade hot-rolled carbon fire-reducing cold heading steel wire rod and manufacturing method thereof
Technical Field
The invention belongs to the technical field of hot-rolled carbon wire rods, and particularly relates to a 10.9-grade hot-rolled carbon fire-reducing cold heading steel wire rod and a manufacturing method thereof.
Background
With the continuous upgrading of the structure of the fastener product to high reinforcement, the proportion of the medium-high strength fastener is continuously improved, the production of the 10.9-grade fastener needs to lead the cold heading steel wire rod to reach the performance grade requirement by multiple drawing, multiple spheroidizing annealing, cold heading forming and quenching and tempering, the spheroidizing annealing adopts the steps of heating the coiled and uncoiled or drawn hot rolled wire rod to austenitizing, and then annealing treatment to spheroidize carbide in the steel to reduce the hardness of the material and improve the cold deformability, but the multiple spheroidizing annealing simultaneously brings the problems of multiple procedures, large emission and high energy consumption. The existing hot rolled wire rod for the 10.9-grade fastener product mainly reaches the aim of high-strength upgrading of the fastener product by adding elements for improving the hardenability of the material, and carbon steel with the alloy elements omitted has the advantages of low material cost and simple smelting, so that the 10.9-grade hot rolled carbon reduced fire cold heading steel wire rod needs to be developed and used for at least reducing one subsequent spheroidizing annealing process so as to meet the market use requirements of green manufacturing of high-strength fastener bolts.
Compared with an alloyed hot-rolled wire rod, the hot-rolled carbon cold heading steel wire rod is difficult to meet the technical difficulty and cause of the 10.9-grade fastener annealing manufacture, and the technical difficulty and cause are as follows:
(1) The existing 10.9-grade hot-rolled cold heading steel wire rod is mainly manufactured by reducing the carbon content affecting the toughness of the wire rod and adding Ti, al, B, mo and other material hardenability elements to ensure the strength grade and combining the cooling control means of a stelmor air cooling line, but the addition of the hardenability elements is easy to cause deterioration plastic tissues such as martensite, bainite and the like in the stelmor air cooling line cooling control process, so that the cracking risk in the cold working process is improved, and in order to achieve the annealing-reducing or annealing-free application, low-temperature wire-laying and slow cooling are adopted to increase the ferrite proportion in the tissues for plastic adjustment after rolling, for example: the patent CN117265408A discloses an annealing-free cold heading steel, a manufacturing method thereof and a fastener obtained by the annealing-free cold heading steel, wherein the composition design of C-Si-Mn-Al-Cr-Mo-B-Mg is adopted, and a low-temperature wire-laying and heat-preserving cooling process at the temperature of less than or equal to 800 ℃ is combined to obtain a ferrite + degenerated pearlite structure, so that Rm is less than or equal to 650MPa, and Z is more than or equal to 53%; on the one hand, after the quenching elements are omitted, in order to ensure the final performance grade, the carbon content is higher than that of alloy steel, so that the problem of increased heat sensitivity of the steel grade is brought, even if a heat preservation cover of a stelmor air cooling line is closed, the wire rod is not completely converted into a ferrite or pearlite austenite structure in the continuous cooling process, and a bainite hard and brittle phase structure still appears at about 500 ℃ at the cooling speed of 2-5 ℃/s, so that the plasticity of the wire rod is obviously reduced; on the other hand, after elements such as Ti, nb and V for inhibiting coarsening of an austenite structure are omitted, grains tend to be coarse at the corresponding heating temperature, along with the improvement of the air cooling speed, wittig body structures which are separated out along crystal faces of saturated solid solutions and distributed in a sheet or needle shape are more likely to appear, the Wittig body structures are high in hardness and extremely poor in plasticity and toughness, the Wittig body structures are difficult to eliminate in the continuous cooling control and temperature reduction process, the inheritance of the structures is accompanied with coarse grains, the risk of cold processing cracking is increased, meanwhile, the highest cooling speed and the total length of a Style mole air cooling line are limited, the abnormal Wittig body is reduced by reducing the cooling speed and preserving heat, the online time of the wire rod is prolonged, the obtained soft-phase ferrite and pearlite structures can cause the production efficiency and the final strength of the cold forging steel wire rod to be too low, the drawing surface-reducing strength-increasing requirement is increased, the plastic loss in the process is larger, and the spheroidizing annealing process is further unfavorable.
(2) In order to reduce the spheroidizing annealing time of carbon cold forging steel, some of the prior art adopts low-temperature rolling to increase the distortion energy in the steel, and utilizes the metastable state of cementite sheets in pearlite, and after the steel is taken off line, cementite is fused and separated out for quick spheroidization, for example: according to the quick spheroidizing medium carbon rod steel and the manufacturing method thereof disclosed in the patent CN116426818A, the C-Si-Mn-Cr-Al-Ca component design is adopted, and the low-temperature heating and the ultralow-temperature rolling are combined to enable the tensile strength to reach 545-582 MPa after short-time spheroidizing, but the strong plasticity is insufficient, so that the cracking risk of the hot rolled wire rod in the process of drawing and cold heading of a 10.9-level fastener is easily increased.
Disclosure of Invention
The invention aims to solve at least one of the technical problems to a certain extent, and provides a 10.9-grade hot-rolled carbon fire-reducing cold heading steel wire rod and a manufacturing method thereof, which are used for designing and efficiently producing and regulating the structure performance of the hot-rolled wire rod based on C-Si-Mn carbon chemical components, particularly improving the plasticity of the cold heading steel wire rod, reducing the cracking risk of cold working caused by abnormal structure, and realizing the green manufacturing of a 10.9-grade high-strength fastener under at least one annealing process so as to meet the market use requirements.
The technical scheme adopted for solving the technical problems is as follows:
A10.9-grade hot-rolled carbon fire-reducing cold heading steel wire rod comprises the following chemical components in percentage by mass: c:0.42% -0.48%, si:0.1% -0.25%, mn: 0.6-0.9%, P is less than or equal to 0.020%, S is less than or equal to 0.020%, and the balance is Fe and unavoidable impurities; the microstructure comprises a mixed structure consisting of 70-76% by volume of tempered pearlite, a small amount of tempered Wittig body and lamellar fused pearlite.
The design basis of the chemical components and the mass percentage of the cold heading steel wire rod comprises:
(1) Carbon: c is the most effective and economic strengthening element in steel, mainly exists in the form of cementite in cold heading steel, can obviously improve the tensile strength of the steel along with the increase of carbon content, but can lead to the increase of cold brittleness and heat sensitivity of the steel, the first eutectoid structure is reduced, and is unfavorable for regulating and controlling the Wittish body structure, so that the purposes of reducing material cost and first precipitating a small amount of Wittish body structure during phase transition are achieved, and the mass percentage of C is controlled to be 0.42% -0.48% on the basis of not adding refined grain elements such as Ti, al, B, mo and other materials hardenability elements, nb, V and the like, so as to ensure the final strength level of the 10.9-level non-regulated fastener.
(2) Silicon: si element is a good deoxidizer, which can improve the hardenability and tensile strength of steel, reduce the critical cooling rate of steel and easily promote the formation of pearlite, but excessive silicon increases the surface decarburization tendency, improves the cold work hardening degree of steel and reduces the cold plastic deformation and toughness of steel, so that the cold heading performance of steel is considered, and the Si content is properly reduced, so that the mass percentage of Si is controlled to be 0.1% -0.25%.
(3) Manganese: mn element is a good deoxidizer and desulfurizer, the strength grade and hardenability of the wire rod can be improved through solid solution strengthening effect, the supercooling degree of austenite during cooling is increased, the method is favorable for refining pearlite and promoting Wittig tissue formation, but the excessive Mn content can aggravate steel segregation, the overheat sensitivity and tempering brittleness tendency of steel are increased, the plasticity and tissue control of steel are both adversely affected, and in order to consider the strength, tissue control and cold working performance of steel, the Mn content is properly improved, so that the mass percentage of Mn is controlled to be 0.6% -0.9%.
(4) Phosphorus, sulfur: the P element and the S element belong to impurity elements, and the segregation at the grain boundary can reduce the toughness of the steel, and the lower the toughness is, the better, so that the P is controlled to be less than or equal to 0.020 percent, and the S is controlled to be less than or equal to 0.020 percent.
On the basis of adopting the carbon steel components with medium C-low Si-high Mn and omitting hardenability elements and bainite, the tempered pearlite in the microstructure retains the characteristics of strength higher than ferrite and plasticity higher than that of pearlite of bainite, the strength of the pearlite structure is further reduced by tempering to improve the toughness, meanwhile, the pearlite with fine lamellar spacing is fused to form lamellar fused pearlite, so as to comprehensively improve the plasticity of the cold heading steel, the tempered wilms utilizes the characteristics of coarser austenite grains of the carbon steel after omitting refined grain elements, the wilms structure is more easily separated out under the conditions of high-temperature carbon diffusion transfer due to a shearing mechanism after cooling, the characteristics of high hardness of the wilms structure are retained, the dislocation density of the wilms structure is obviously reduced by tempering to improve the toughness energy of the plastic, and the strong and tough structure property is obtained, compared with the prior art that the strength of the wire rod is improved by refining grains after adding the hardenability element, the cold heading steel wire rod is mainly provided with tempered pearlite, a small amount of tempered Wittig body is used for providing matrix strength, the strength loss of a later strip of the hardenability element is compensated, compared with the prior art that the plasticity of the wire rod is improved by increasing the ferrite proportion in a structure or annealing is simplified by utilizing the metastable state of pearlite sheets, the tempered state structure of the cold heading steel wire rod with pearlite and Wittig body structure is improved and eliminated by internal stress, the structure stability is improved, the brittleness is obviously improved, a small amount of sheet-layer fused pearlite is combined, the high-plasticity heading steel wire rod can be obtained while the wire rod strength is considered, the annealing difficulty is reduced by reducing the dislocation density of the structure and the spheroidizing of the sheet-layer fused pearlite, at least one spheroidizing annealing procedure is reduced when the cold heading steel wire rod is used for the subsequent manufacture of 10.9-level fasteners, has good market application prospect.
Preferably, the finer the lamellar spacing of the tempered pearlite is, the strength of the cold heading steel wire rod is increased, and the plasticity is reduced, so that the lamellar spacing of the tempered pearlite can be further controlled to be 75-100 nm, and the strength and the plasticity of the cold heading steel wire rod can be regulated and controlled.
Preferably, the higher the proportion of the tempered Wittig body is, the strength and plasticity of the cold heading steel wire rod are improved, so that the volume percentage of the tempered Wittig body can be further controlled to be 22% -28%, and the strength and plasticity of the cold heading steel wire rod can be regulated and controlled.
Preferably, the cold heading steel wire rod has the diameter of 6.5-18.0 mm, the tensile strength of 880-910 MPa and the reduction of area of 57% -61%, has the high-strength characteristic which is not inferior to that of an alloyed steel, has the obviously improved plasticity characteristic compared with an air-cooled wire rod with ferrite and pearlite structure, and has higher reduction of area, so that the cold heading steel wire rod can be used for manufacturing application fields such as 10.9-level high-strength fastener bolts, and at least one spheroidizing annealing process is reduced.
The manufacturing method of the 10.9-grade hot rolled carbon reduced fire cold heading steel wire rod comprises the following steps:
Based on the chemical components of the 10.9-grade hot-rolled carbon fire-reducing cold heading steel wire rod, wire rods are spun into wire rods according to the spinning temperature of more than or equal to 960 ℃, the wire rods are subjected to weak isothermal in an online salt bath, the wire rods are cooled to the molten salt temperature according to the cooling speed of more than or equal to 36 ℃/s, high-temperature austenite in the wire rod tissue is converted into fine lamellar-spacing pearlite and a small amount of Wig's body, isothermal tempering is simultaneously converted into tempered pearlite and tempered Wig's body, and lamellar melting of the pearlite is promoted to form lamellar melting pearlite, and finally the sheet melting pearlite is subjected to rapid cooling through a roller way, so that the cold heading steel wire rod with a microstructure comprising a mixed structure consisting of 70% -76% by volume percent of tempered pearlite, a small amount of tempered Wig's body and lamellar melting pearlite is prepared.
The manufacturing method adopts C-Si-Mn component, properly coarsens austenite grains at higher spinning temperature, is easier to obtain a higher proportion of Wittig body tissue, the wire rod after Wen Tu wires is directly subjected to online salt bath weak isothermal treatment through molten salt, compared with the prior Steyr air cooling wire, the wire rod can quickly skip the phase transition temperature range of ferrite at higher cooling speed and higher supercooling degree, compared with the strong isothermal treatment with lower temperature and longer time, on the basis of carbon steel component, the online salt bath weak isothermal treatment can avoid precipitation of bainite or martensite tissue, so that most of high-temperature austenite in the wire rod tissue after spinning is converted into pearlite with fine lamellar spacing, A small part of high-temperature austenite forms a needle-shaped Wittig body tissue under the high-temperature carbon diffusion transfer condition, so that the strength of a matrix is provided, meanwhile, compared with the existing heat preservation cooling or delay cooling process, the high-temperature isothermal state of a wire rod is maintained for a longer time by utilizing the high heat exchange capability of molten salt, the pearlite is tempered to form tempered pearlite, meanwhile, the pearlite with fine lamellar spacing is easily fused to form lamellar pearlite, the dislocation density of the Wittig body tissue is reduced to form tempered Wittig body, compared with the online salt bath weak isothermal treatment method adopting a two-stage salt bath treatment process of respectively low temperature and high temperature, the control of the molten salt temperature is simpler and more convenient, and the state of the fine lamellar spacing of the tempered pearlite is also easily maintained, so that excessive tempering and softening are avoided.
As the austenite structure in the wire rod structure is fully transformed after the online salt bath is weakly isothermal, the condition that the structural uniformity is affected by the hard and brittle phases separated out in the roller way rapid cooling process due to the increased carbon content of carbon steel is avoided, the wire rod reaches a coil collecting position rapidly through the roller way rapid cooling process, the online time can be effectively reduced, the production efficiency of the cold heading steel wire rod is improved, meanwhile, the wire rod is rapidly cooled through the roller way rapid cooling process, the excessive tempering softening of the wire rod is prevented, the strength grade of the wire rod is reduced, the structure, the strength and the plasticity matching of the carbon cold heading steel wire rod are finally regulated and controlled, and the method is more beneficial to simplifying the manufacturing links and reducing the production cost.
Preferably, the condition of abnormal structures of Wittig bodies and bainite is improved by adopting online salt bath weak isothermal treatment after spinning, isothermal treatment for a longer time can be obtained by adopting relative heat preservation and cooling, and the problem of increased abrasion of a rolling line caused by low-temperature rolling is not needed to be considered for increasing the ferrite ratio, so that the wire rod is produced by adopting hot rolling, the final rolling temperature is controlled to 980-1010 ℃, the final rolling reduction is 26-36%, the grain size of the wire rod is less than or equal to 8 grades, on one hand, the abrasion on the rolling line can be reduced by using a higher final rolling temperature, the rolling efficiency is improved, and on the other hand, wire rod grains can be properly coarsened by using a higher final rolling temperature and a large final rolling reduction, and the wire rod grains with proper proportion of pearlite and Wittig bodies can be used as preparation on the structure after spinning.
Preferably, the higher the wire laying temperature is, the higher the tempered Wipe body ratio in the tissue is, whereas the lower the wire laying temperature is, the higher the tempered pearlite ratio in the tissue is, therefore, the wire rod laying temperature can be further regulated to regulate the matrix strength, and the wire laying temperature is preferably less than or equal to 980 ℃.
Preferably, since the carbon cold-headed steel wire rod is manufactured for the purposes of high-efficiency production of cold-headed steel wire rods and reduced annealing production of 10.9-grade fasteners, the lower the isothermal temperature is, the shorter the isothermal treatment time is, the finer the lamellar spacing of tempered pearlite is, so that the strength and plasticity of the cold-headed steel wire rod are improved, but the lower the isothermal temperature is, the bainitic structure and even the martensitic structure can appear, the obvious strength loss is caused, the lower the isothermal treatment time is, the pearlite and the Wittier body are not completely tempered, so that the brittleness of the cold-headed steel wire rod is obviously improved, otherwise, the higher the isothermal temperature is, the longer the isothermal treatment time is, the thicker the lamellar spacing of tempered pearlite is, the lamellar pearlite energy storage is increased, the lamellar fused pearlite ratio is increased with the extension of the isothermal treatment time, the strength and plasticity of the cold-headed steel wire rod are improved, however, the larger lamellar spacing of pearlite generated by excessively high isothermal temperature can lead to larger lamellar spacing of tempered pearlite, is not beneficial to fusing to form lamellar pearlite, is unfavorable for plasticity of cold heading steel wire rods, even ferrite tissues can appear when the isothermal temperature is higher, the strength of the cold heading steel wire rods is unfavorable, the energy consumption and the online time are increased when the isothermal treatment time is excessively long, the efficient production is unfavorable, meanwhile, the lamellar spacing of the tempered pearlite is increased, the wire rods are excessively tempered and softened, the strength grade of the wire rods is reduced, therefore, the isothermal temperature and the isothermal treatment time of weak isothermal in online salt bath can be further regulated, preferably, the isothermal temperature of weak isothermal in online salt bath is controlled at 525-555 ℃, and the isothermal treatment time is controlled at 30-230 s, so that the strength and the plasticity of the wire rods are regulated and matched.
Preferably, the wire rod is quickly reduced to lower molten salt temperature after entering molten salt from higher spinning temperature, the temperature difference is larger, preferably, the front end of the online weak isothermal salt bath is controlled to control the circulating amount of the molten salt to be 450-650 t/h, the temperature rise of the molten salt is less than or equal to 8 ℃, isothermal transformation of the wire rod in a target temperature range is controlled by preventing the temperature rise from being too high, and the volume fraction of each phase of the wire rod is regulated and controlled.
Preferably, the back end of the online salt bath weak isothermal salt bath is controlled to control the circulation quantity of molten salt to be 250-450 t/h, the temperature rise of the molten salt is less than or equal to 3 ℃, and the weak isothermal treatment can be completed by controlling the wire rod within a target temperature range so as to regulate and control the strength and plasticity matching of the wire rod.
Preferably, the cooling speed of the roller way rapid cooling control wire rod is 3-6 ℃/s, the wire rod is controlled to be collected below 450 ℃, the wire rod can rapidly reach a collecting position at a higher cooling speed under the cooling speed, excessive softening caused by excessively low cooling speed is prevented from reducing the strength of cold heading steel wire rods, and meanwhile, excessive hardening and increasing collecting difficulty caused by excessively low temperature of the wire rod reaching the collecting position due to excessively high cooling speed are avoided, so that the cooling speed of the roller way rapid cooling can be further controlled, and the high-efficiency production and the same circle degree of coiling after the wire rod is collected are both considered.
Preferably, the roller way is rapidly cooled by adopting a heat preservation cover to open or simultaneously opening a fan according to 15% -40% of the total air quantity, the total air quantity of the fan is 16-26 ten thousand m 3/h, the roller way is used for conveying the wire rod according to the roller way speed of 0.9-1.6 m/s, and the cooling speed of the wire rod is controlled by air cooling or weak air cooling, so that the high-efficiency production of cold heading steel wire rods is facilitated.
Compared with the prior art, the invention has the beneficial effects that:
(1) Aiming at the current situation that the cracking risk of the hot rolled wire rod in the fastener drawing and cold heading processes is easily improved due to hardenability elements and abnormal structures, the 10.9-grade hot rolled carbon reduced fire cold heading steel wire rod adopts C-Si-Mn carbon chemical composition design, the microstructure type comprises a mixed structure which is mainly tempered pearlite, a small amount of strong and tough tempered Wittig bodies and lamellar fused pearlite, the pearlite and Wittig bodies are used for providing matrix strength, the plasticity of the pearlite structure and the Wittig bodies is improved by tempering, the lamellar fused pearlite is used for improving the plasticity, the annealing difficulty is reduced, the occurrence of bainite abnormal structure is avoided, the tensile strength of the product is 880-910 MPa, the area shrinkage is 57% -61%, the microstructure type hot rolled wire rod is used for manufacturing 10.9-grade high strength fastener bolts and other application fields, at least one annealing procedure can be reduced, and the microstructure hot rolled wire rod has good market application prospect.
(2) Aiming at the current situation that the existing hot rolled wire rod for the fastener product is easy to generate abnormal structure, yield and low production efficiency by adding elements for improving the hardenability of the material and combining the cooling control means of a stelmor air cooling line, the manufacturing method of the 10.9-grade hot rolled carbon reduced fire cold heading steel plate adopts the C-Si-Mn carbon chemical composition design and the online salt bath weak isothermal and roller way rapid cooling technology design, can promote the high-temperature austenite in the wire rod structure to be converted into pearlite with fine lamellar spacing and a small amount of Wittig body, and simultaneously, the isothermal tempering is converted into tempered pearlite and tempered Wittig body, so that the lamellar melting of the pearlite forms lamellar fusing pearlite, the hot rolled wire rod structure strong plasticity is rapidly produced and regulated, and particularly, the cold heading steel wire rod plasticity is improved, the wire rod is prevented from excessively tempering softening, the manufacturing method is simplified, the online time is reduced, the manufacturing efficiency is obviously improved, and the industrial applicability is good.
Drawings
The foregoing and/or additional aspects and advantages of the invention will become apparent and may be better understood from the following description of embodiments taken in conjunction with the accompanying drawings in which:
FIG. 1 is a metallographic structure diagram of example 1 of the present invention;
FIG. 2 is a metallographic structure diagram of example 3 of the present invention;
FIG. 3 is a metallographic structure of comparative example 6 of the present invention.
Detailed Description
The embodiments described below are exemplary only and are not intended to limit the description of the features and characteristics of the invention, in order to set forth the best mode of carrying out the invention, intended to illustrate it and to enable those skilled in the art to practice it, without any limitation to its scope, which is defined solely by the claims appended hereto.
Example 1:
The 10.9-grade hot-rolled carbon fire-reducing cold heading steel wire rod comprises the following chemical components in percentage by mass: c:0.45%, si:0.2%, mn:0.9%, P:0.02%, S:0.019%, the balance being Fe and unavoidable impurities; the manufacturing method comprises the following steps of hot rolling, high-temperature wire laying, on-line salt bath weak isothermal, roller way quick cooling and coil collecting, and specifically comprises the following steps of:
The hot rolling procedure is used for heating a billet with the specification of 160mm multiplied by 160mm through a heating furnace to obtain a high-temperature billet with rolling plasticity, rapidly rolling a wire rod with the specification of 6.5mm through a rolling line at high temperature, reducing the abrasion of a rolling mill of the rolling line, improving the rolling efficiency, and simultaneously properly coarsening wire rod grains with higher final rolling temperature and large final rolling reduction, so as to obtain pearlite and Wittig body with proper proportions for preparation on a structure after spinning, and is specific: controlling the final rolling temperature to be 987 ℃, controlling the final rolling reduction to be 36%, and controlling the grain size of the wire rod to be less than or equal to 8 grades; the high-temperature wire spinning procedure is used for making wires which are discharged from a rolling line into wire rods through a wire spinning machine, controlling the wire spinning temperature to 965 ℃, dispersing the wire rods on a roller way and conveying the wire rods along the roller way, and using higher wire spinning temperature to properly coarsen austenite grains of the wire rod structure, so that a higher-proportion Wittig body structure is easier to obtain.
The online salt bath weak isothermal method comprises the steps of adopting a salt bath tank with molten salt arranged therein, conveying the wire rods after spinning to pass through the molten salt of the salt bath tank through a roller way, enabling the wire rods to be cooled down to the temperature of the molten salt at a cooling speed of 39 ℃/s, rapidly skipping a ferrite transformation temperature interval at a higher cooling speed, enabling high-temperature austenite in a wire rod tissue to be transformed into pearlite with fine lamellar spacing and a small amount of Wittig body, simultaneously enabling isothermal tempering to be transformed into tempered pearlite and tempered Wittig body, enabling pearlite lamellar fusing to form lamellar fusing pearlite, preventing the temperature rise of the molten salt from being too high in the process, and controlling the wire rods to complete isothermal transformation within a target temperature range, and specifically: the isothermal temperature is controlled at 525 ℃, the isothermal treatment time is controlled at 30s, the front end of the salt bath is controlled to control the molten salt circulation amount to be 600t/h, the molten salt temperature rise is less than or equal to 8 ℃, the rear end of the salt bath is controlled to control the molten salt circulation amount to be 450t/h, and the molten salt temperature rise is less than or equal to 3 ℃.
The roller way quick cooling procedure carries out quick cooling treatment with the wire rod that comes out from the salt bath, prevents that the wire rod from excessively tempering and softening and reducing wire rod intensity level, adjusts and controls the intensity and the plasticity of cold heading steel wire rod to match, and is specific: the heat preservation cover is opened, the coil rod coming out of the salt bath is conveyed by a roller way at the speed of 0.9m/s, and the cooling speed of the coil rod is controlled to be 3 ℃/s until the coil rod is conveyed to a coil collecting station; the coil collecting procedure is used for collecting the coil rod into coils through a coil collecting drum, the coil collecting temperature is 405 ℃, and the cold heading steel coil rod finished product is obtained after packaging and warehousing, and the metallographic structure diagram of the cold heading steel coil rod finished product is shown in figure 1.
Comparative example 1:
A manufacturing method of a hot-rolled carbon cold heading steel wire rod is different from example 1 in that: the manufacturing method comprises the following steps of low-temperature controlled rolling, low-temperature wire laying, heat preservation and cooling, and coil collecting, and specifically comprises the following steps of: the final rolling temperature of the low-temperature controlled rolling process is 900 ℃, the grain size of the rolled wire rod is 9 grade, the wire laying temperature of the low-temperature wire laying process is 870 ℃, the wire rod after wire laying is conveyed into a heat insulation cover through a roller way for heat insulation slow cooling, the phase change is completed in the cover at the cooling speed of 2.1 ℃/s, the coil collecting temperature is 400 ℃, and the cold heading steel wire rod is obtained after coil collecting and discharging.
Comparative example 2:
A manufacturing method of a hot-rolled carbon cold heading steel wire rod is different from example 1 in that: the manufacturing method comprises the following steps of hot rolling, high-temperature wire laying, stelmor air cooling, roller way slow cooling and coil collecting, and specifically comprises the following steps of: the method comprises the steps of feeding a wire rod subjected to wire spinning into a Steyr air cooling line, controlling a1 # fan to 4# fan with the total air quantity of 20 ten thousand m 3/h to be started according to 75%, enabling the wire rod to be cooled to 670 ℃ at the cooling speed of 7.5 ℃/s, closing a roller way slow cooling device and a heat preservation cover, conveying the wire rod subjected to the Steyr air cooling by a roller way according to the roller way of 1.3m/s, controlling the cooling speed of the wire rod to be 0.9 ℃/s, and obtaining the cold heading steel wire rod after the wire rod is wound to a winding station until the wire rod is conveyed to the winding station, the winding temperature is 410 ℃.
Example 2:
The 10.9-grade hot-rolled carbon fire-reducing cold heading steel wire rod comprises the following chemical components in percentage by mass: c:0.48%, si:0.1%, mn:0.6%, P:0.018%, S:0.018%, the balance being Fe and unavoidable impurities; the manufacturing method comprises the following steps of hot rolling, high-temperature wire laying, on-line salt bath weak isothermal, roller way quick cooling and coil collecting, and specifically comprises the following steps of:
The hot rolling procedure is used for heating a billet with the specification of 160mm multiplied by 160mm through a heating furnace to obtain a high-temperature billet with rolling plasticity, rapidly rolling the billet into a wire with the specification of 10mm through a rolling line at high temperature, reducing the wear of a rolling mill of the rolling line, improving the rolling efficiency, and simultaneously properly coarsening wire grains with higher final rolling temperature and large final rolling reduction, so as to obtain pearlite and Wittig body with proper proportions on a tissue after spinning, and is specific: controlling the final rolling temperature to 1010 ℃, the final rolling reduction to 32%, and the grain size of the wire rod to be less than or equal to 8 grades; the high-temperature wire spinning procedure is used for making wires which are discharged from a rolling line into wire rods through a wire spinning machine, controlling the wire spinning temperature to be 980 ℃, dispersing the wire rods on a roller way and conveying the wire rods along the roller way, and using a higher wire spinning temperature to properly coarsen austenite grains of the wire rod structure, so that a higher-proportion Wittig body structure is easier to obtain.
The online salt bath weak isothermal method comprises the steps of adopting a salt bath tank with molten salt arranged therein, conveying the wire rods after spinning to pass through the molten salt of the salt bath tank through a roller way, enabling the wire rods to be cooled to the molten salt temperature at a cooling speed of 40 ℃/s, rapidly skipping a ferrite transformation temperature interval at a faster cooling speed, enabling high-temperature austenite in a wire rod tissue to be transformed into pearlite with fine lamellar spacing and a small amount of Wittig body, simultaneously enabling isothermal tempering to be transformed into tempered pearlite and tempered Wittig body, enabling pearlite lamellar fusing to form lamellar fusing pearlite, preventing the molten salt from rising too high in temperature in the process, and controlling the wire rods to complete isothermal transformation within a target temperature range, and specifically: the isothermal temperature is controlled at 532 ℃, the isothermal treatment time is controlled at 95s, the front end of the salt bath is controlled to control the molten salt circulation quantity to be 650t/h, the molten salt temperature rise is less than or equal to 8 ℃, the rear end of the salt bath is controlled to control the molten salt circulation quantity to be 370t/h, and the molten salt temperature rise is less than or equal to 3 ℃.
The roller way quick cooling procedure carries out quick cooling treatment with the wire rod that comes out from the salt bath, prevents that the wire rod from excessively tempering and softening and reducing wire rod intensity level, adjusts and controls the intensity and the plasticity of cold heading steel wire rod to match, and is specific: the heat preservation cover is adopted to be opened, meanwhile, a 11 # 14 fan with the total air quantity of 16 ten thousand m 3/h is started according to 40% of the total air quantity, a roller way is used for conveying the wire rods from the salt bath at the roller way speed of 1.4m/s, and the cooling speed of the wire rods is controlled to be 4.5 ℃/s until the wire rods are conveyed to a coil collecting station; the coil collecting procedure is used for collecting the coil rod into coils through a coil collecting drum, the coil collecting temperature is 416 ℃, and the cold heading steel coil rod finished product is obtained after packaging and warehousing.
Comparative example 3:
a manufacturing method of a hot-rolled carbon cold heading steel wire rod, which is different from example 2 in that: and the final rolling temperature is 950 ℃, the wire laying temperature is 930 ℃, and the cold heading steel wire rod is obtained after coil collecting and wire discharging.
Comparative example 4:
A manufacturing method of a hot-rolled carbon cold heading steel wire rod, which is different from example 2 in that: and the final rolling temperature is 1025 ℃, the wire laying temperature is 995 ℃, and the cold heading steel wire rod is obtained after coil collecting and coil discharging.
Example 3:
The 10.9-grade hot-rolled carbon fire-reducing cold heading steel wire rod comprises the following chemical components in percentage by mass: c:0.46%, si:0.15%, mn:0.73%, P:0.018%, S:0.019%, the balance being Fe and unavoidable impurities; the manufacturing method comprises the following steps of hot rolling, high-temperature wire laying, on-line salt bath weak isothermal, roller way quick cooling and coil collecting, and specifically comprises the following steps of:
The hot rolling procedure is used for heating a billet with the specification of 220mm multiplied by 220mm through a heating furnace to obtain a high-temperature billet with rolling plasticity, rapidly rolling the billet into a wire with the specification of 18mm at high temperature through a rolling line, reducing the wear of a rolling mill of the rolling line, improving the rolling efficiency, and simultaneously properly coarsening wire grains with higher final rolling temperature and large final rolling reduction, so as to obtain pearlite and Wittig body with proper proportions on a tissue after spinning, and is specific: controlling the final rolling temperature to 992 ℃, the final rolling reduction to 26%, and the grain size of the wire rod is less than or equal to 8 grades; the high-temperature wire spinning procedure is used for making wires which are discharged from a rolling line into wire rods through a wire spinning machine, controlling the wire spinning temperature to be 970 ℃, dispersing the wire rods on a roller way and conveying the wire rods along the roller way, and using higher wire spinning temperature to properly coarsen austenite grains of the wire rod structure, so that a higher-proportion Wittig body structure is easier to obtain.
The online salt bath weak isothermal method comprises the steps of adopting a salt bath tank with molten salt arranged therein, conveying the wire rods after spinning to pass through the molten salt of the salt bath tank through a roller way, enabling the wire rods to be cooled to the molten salt temperature at a cooling speed of 37 ℃/s, rapidly skipping a ferrite transformation temperature interval at a faster cooling speed, enabling high-temperature austenite in a wire rod tissue to be transformed into pearlite with fine lamellar spacing and a small amount of Wittig body, simultaneously enabling isothermal tempering to be transformed into tempered pearlite and tempered Wittig body, enabling pearlite lamellar fusing to form lamellar fusing pearlite, preventing the molten salt from rising too high in temperature in the process, and controlling the wire rods to complete isothermal transformation within a target temperature range, and specifically: the isothermal temperature is controlled at 555 ℃, the isothermal treatment time is controlled at 230s, the front end of the salt bath is controlled to control the molten salt circulation amount to be 520t/h, the molten salt temperature rise is less than or equal to 8 ℃, the rear end of the salt bath is controlled to control the molten salt circulation amount to be 250t/h, and the molten salt temperature rise is less than or equal to 3 ℃.
The roller way quick cooling procedure carries out quick cooling treatment with the wire rod that comes out from the salt bath, prevents that the wire rod from excessively tempering and softening and reducing wire rod intensity level, adjusts and controls the intensity and the plasticity of cold heading steel wire rod to match, and is specific: the heat preservation cover is adopted to be opened, meanwhile, a 11 # 14 fan with the total air quantity of 26 ten thousand m 3/h is started according to 15% of the total air quantity, a roller way is used for conveying the wire rods coming out of the salt bath at the roller way speed of 1.6m/s, and the cooling speed of the wire rods is controlled to be 6 ℃/s until the wire rods are conveyed to a coil collecting station; the coil collecting procedure is used for collecting the coil rod into coils through a coil collecting drum, the coil collecting temperature is 420 ℃, and the cold heading steel coil rod finished product is obtained after packaging and warehousing, and the metallographic structure diagram of the cold heading steel coil rod finished product is shown in figure 2.
Comparative example 5:
a manufacturing method of a hot-rolled carbon cold heading steel wire rod, which is different from example 3 in that: the isothermal temperature is controlled at 500 ℃, the isothermal treatment time is controlled at 85s, and the cold heading steel wire rod is obtained after coil collecting and off-line.
Comparative example 6:
a manufacturing method of a hot-rolled carbon cold heading steel wire rod, which is different from example 3 in that: the isothermal temperature is controlled at 25 ℃, and after coil collection and coil dropping, a cold heading steel wire rod is obtained, and a metallographic structure diagram of the cold heading steel wire rod is shown in figure 3.
Comparative example 7:
A manufacturing method of a hot-rolled carbon cold heading steel wire rod, which is different from example 3 in that: the isothermal temperature is controlled at 565 ℃, the isothermal treatment time is controlled at 450s, and the cold heading steel wire rod is obtained after coil collecting and off-line.
Example 4:
The 10.9-grade hot-rolled carbon fire-reducing cold heading steel wire rod comprises the following chemical components in percentage by mass: c:0.42%, si:0.25%, mn:0.82%, P:0.02%, S:0.02% of Fe and the balance of unavoidable impurities; the manufacturing method comprises the following steps of hot rolling, high-temperature wire laying, on-line salt bath weak isothermal, roller way quick cooling and coil collecting, and specifically comprises the following steps of:
The hot rolling procedure is used for heating a billet with the specification of 220mm multiplied by 220mm through a heating furnace to obtain a high-temperature billet with rolling plasticity, rapidly rolling the billet into a wire rod with the specification of 14mm at high temperature through a rolling line, reducing the wear of a rolling mill of the rolling line, improving the rolling efficiency, and simultaneously properly coarsening wire crystal grains with higher final rolling temperature and large final rolling reduction, so as to obtain pearlite and Wittig body with proper proportions on a tissue after spinning, and specifically: controlling the final rolling temperature to 980 ℃, controlling the final rolling reduction to 28%, and controlling the grain size of the wire rod to be less than or equal to 8 grades; the high-temperature wire spinning procedure is used for making wires which are discharged from a rolling line into wire rods through a wire spinning machine, controlling the wire spinning temperature to 960 ℃, dispersing the wire rods on a roller way and conveying the wire rods along the roller way, and using a higher wire spinning temperature to properly coarsen austenite grains of the wire rod structure, so that a higher-proportion Wittig body structure is easier to obtain.
The online salt bath weak isothermal method comprises the steps of adopting a salt bath tank with molten salt arranged therein, conveying the wire rods after spinning to pass through the molten salt of the salt bath tank through a roller way, enabling the wire rods to be cooled to the molten salt temperature at a cooling speed of 36 ℃/s, rapidly skipping a ferrite transformation temperature interval at a faster cooling speed, enabling high-temperature austenite in a wire rod tissue to be transformed into pearlite with fine lamellar spacing and a small amount of Wittig body, simultaneously enabling isothermal tempering to be transformed into tempered pearlite and tempered Wittig body, enabling pearlite lamellar fusing to form lamellar fusing pearlite, preventing the molten salt from rising too high in temperature in the process, and controlling the wire rods to complete isothermal transformation within a target temperature range, and specifically: the isothermal temperature is controlled at 546 ℃, the isothermal treatment time is controlled at 170s, the front end of the salt bath is controlled to control the molten salt circulation quantity to be 450t/h, the molten salt temperature rise is less than or equal to 8 ℃, the rear end of the salt bath is controlled to control the molten salt circulation quantity to be 290t/h, and the molten salt temperature rise is less than or equal to 3 ℃.
The roller way quick cooling procedure carries out quick cooling treatment with the wire rod that comes out from the salt bath, prevents that the wire rod from excessively tempering and softening and reducing wire rod intensity level, adjusts and controls the intensity and the plasticity of cold heading steel wire rod to match, and is specific: the heat preservation cover is adopted to be opened, meanwhile, a 11 # 14 fan with the total air quantity of 20 ten thousand m 3/h is started according to 30% of the total air quantity, a roller way is used for conveying the wire rods from the salt bath at the roller way speed of 1.2m/s, and the cooling speed of the wire rods is controlled to be 5.2 ℃/s until the wire rods are conveyed to a coil collecting station; the coil collecting procedure is used for collecting the coil rod into coils through a coil collecting drum, the coil collecting temperature is 390 ℃, and the cold heading steel coil rod finished product is obtained after packaging and warehousing.
Comparative example 8:
A manufacturing method of a hot-rolled carbon cold heading steel wire rod, which is different from example 4 in that: the manufacturing method comprises the following steps of hot rolling, high-temperature wire laying, on-line salt bath weak isothermal, roller way slow cooling and coil collecting, and specifically comprises the following steps of: and the roller way slow cooling is closed by adopting a fan and a heat preservation cover, the roller way is used for conveying the coil rod subjected to the stelmor air cooling according to the roller way of 0.4m/s, the cooling speed of the coil rod is controlled to be 1.2 ℃/s until the coil rod is conveyed to a coil collecting station, the coil collecting temperature is 438 ℃, and the cold heading steel coil rod is obtained after coil collecting and discharging.
Comparative example 9:
A manufacturing method of a hot-rolled carbon cold heading steel wire rod, which is different from example 4 in that: the manufacturing method comprises the following steps of hot rolling, high-temperature wire laying, on-line salt bath weak isothermal, roller way slow cooling and coil collecting, and specifically comprises the following steps of: the roller way quick cooling process adopts a warm cover to be started, meanwhile, a 11 # 14 fan with the total air quantity of 20 ten thousand m 3/h is started according to 65% of the total air quantity, a roller way is used for conveying a wire rod coming out of a salt bath at the speed of the roller way of 1.1m/s, and the cooling speed of the wire rod is controlled to be 7.2 ℃/s until the wire rod is conveyed to a coil collecting station; and the coil collecting temperature is 310 ℃, and the cold heading steel wire rod is obtained after coil collecting and offline.
The cold heading steel wire rods obtained in the examples and the comparative examples are subjected to structure and performance detection: tensile testing was performed using the metal material tensile test section 1 of GB-T228.1-2021: room temperature test method, to obtain tensile strength and reduction of area, and to perform tissue detection according to the metal microstructure detection method of GB/T13298 standard, the comparison results obtained are shown in table 1 below:
TABLE 1 comparison of the composition of the steel wire rods of the different Cold heading and the properties of the wire rod structure of the manufacturing method
As can be seen from the comparison results of examples 1-4 and comparative example 1, compared with the carbon steel type, the low-temperature wire laying and heat-preserving cooling process combined with the prior stelmor air cooling line still has a bainite abnormal structure, and on the basis of adopting the carbon steel components with medium C-low Si-high Mn and omitting hardenability elements and elements, the high-temperature austenite in the wire rod structure is promoted to be converted into fine lamellar spacing pearlite and a small amount of Wildshi body, the fine lamellar spacing pearlite and the small amount of Wildshi body are subjected to isothermal tempering, the fine lamellar spacing pearlite and the small amount of Wildshi body are converted into tempered pearlite and tempered Wildshi body, and meanwhile, the lamellar melting of the pearlite is promoted to form lamellar melting pearlite, so that the condition that the structural uniformity is influenced due to the fact that the hard and brittle phases are separated out in the roller way rapid cooling process due to the fact that the carbon content is increased can be avoided.
As can be seen from the comparison results of examples 1-4 and comparative example 2, compared with the carbon steel, the rapid air cooling and slow cooling process of the prior stelmor air cooling line under the combination of high temperature spinning can obviously increase the brittleness of the cold heading steel wire rod due to the occurrence of Wittig body tissues which are separated out along crystal faces of saturated solid solutions and distributed in a sheet shape or a needle shape, the invention obviously reduces the dislocation density of the Wittig body tissues by tempering to improve the plastic toughness energy, obtains strong and tough tempered Wittig body tissues, mainly uses tempered pearlite and provides matrix strength by a small amount of tempered Wittig body, the method makes up the strength loss of the quenching elements in the subsequent zone, improves the internal stress of the structure and the stability of the structure by using a tempered structure, combines a small amount of lamellar fused pearlite formed by fusing the lamellar fused pearlite to improve the plasticity and reduce the annealing difficulty, can reach the tensile strength of products of 880-910 MPa and the reduction of area of 57-61 percent, is used for the application fields of manufacturing 10.9-level high-strength fastener bolts and the like, can at least reduce one annealing process, and has good market application prospect.
As can be seen from the comparison results of examples 1-4 and comparative example 3, the lower the spinning temperature is, the lower the tempered Winter body ratio in the tissue is, the strength of the cold heading steel wire rod is reduced, and the plasticity is increased; as can be seen from the comparison of examples 1-4 and comparative example 4, the higher the spinning temperature, the higher the tempered Wittig body ratio in the tissue, and the further the wire rod spinning temperature can be controlled to control the ratio of tempered pearlite to tempered Wittig body.
As can be seen from the comparison results of examples 1 to 4 and comparative example 5, the lower the isothermal temperature and the shorter the isothermal treatment time, the finer the lamellar spacing of tempered pearlite is, so that the strength and plasticity of the cold heading steel wire rod are improved, but as can be seen from the comparison results of examples 1 to 4 and comparative example 6, even the quenched martensitic structure can appear when the isothermal temperature is too low, and the plasticity is obviously lost; as can be seen from the comparison results of examples 1-4 and comparative example 7, the higher the isothermal temperature, the thicker the lamellar spacing of the tempered pearlite is, so that the strength of the cold-headed steel wire rod is reduced and the plasticity is increased, but the lamellar spacing of the tempered pearlite generated by the excessively high isothermal temperature is larger, and is also unfavorable for fusing to form lamellar pearlite, and the longer the isothermal treatment time is, the proportion of lamellar fused pearlite is increased, so that the strength of the cold-headed steel wire rod is reduced and the plasticity is increased, and the isothermal temperature and the isothermal treatment time of weak isothermal in an online salt bath can be further regulated and controlled to regulate the strength and the plasticity matching of the wire rod.
As can be seen from the comparison results of examples 1-4 and comparative example 8, compared with the slow cooling of the roller way, the rapid cooling of the roller way can enable the wire rod to reach the coil collecting position rapidly at a rapid cooling speed, so that the strength of the cold heading steel wire rod is prevented from being reduced due to excessive softening caused by the excessively low cooling speed; as can be seen from the comparison between examples 1-4 and comparative example 9, although the improvement of the cooling rate of the roller way rapid cooling process can improve the production efficiency, the too high cooling rate can cause too low temperature of the coil rod reaching the coil collecting position to harden excessively, so that the coil misplacement is serious, and the packaging and transportation are unfavorable.
The above list of detailed descriptions is only specific to practical embodiments of the present invention, and they are not intended to limit the scope of the present invention, for example: the billet before hot rolling can be produced by adopting the process flows of converter smelting, refining and continuous casting, and all equivalent embodiments or changes which do not depart from the technical spirit of the invention are included in the protection scope of the invention.