CN117581396B - A lithium iron phosphate composite material, its preparation method and applications - Google Patents
A lithium iron phosphate composite material, its preparation method and applicationsInfo
- Publication number
- CN117581396B CN117581396B CN202380011170.7A CN202380011170A CN117581396B CN 117581396 B CN117581396 B CN 117581396B CN 202380011170 A CN202380011170 A CN 202380011170A CN 117581396 B CN117581396 B CN 117581396B
- Authority
- CN
- China
- Prior art keywords
- lithium
- iron phosphate
- source
- lithium iron
- porous
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Active
Abstract
The present disclosure provides a lithium iron phosphate composite material, a preparation method and an application thereof, wherein the preparation method is to mix porous inorganic nanofiber aerogel, a lithium source, an iron source, a phosphorus source and a carbon source to obtain a dispersion, spray-dry the dispersion to obtain a precursor, and then sinter the precursor to obtain the lithium iron phosphate composite material. The porous inorganic nanofiber aerogel is used for in-situ compounding of lithium iron phosphate while the lithium iron phosphate is synthesized, the porous nanofiber enables lithium iron phosphate particles to be distributed more uniformly and not to be agglomerated any more, the double effects of the porous nanofiber and the aerogel can effectively shorten the transmission path of Li + and effectively improve the multiplying power performance of the obtained material, meanwhile, the porous inorganic nanofiber aerogel can play a supporting role, damage caused by processing processes such as pressing is avoided, the volume change of the obtained material during charging and discharging is relieved, the problems such as cracking are avoided, and the stability of the material is improved.
Description
Technical Field
The disclosure belongs to the field of batteries, and relates to a positive electrode material, in particular to a lithium iron phosphate composite material, and a preparation method and application thereof.
Background
Secondary Lithium Ion Batteries (LIBs) have been attracting attention and realizing commercial applications in a plurality of fields due to the advantages of high operating voltage and energy density, particularly low toxicity and environmental friendliness of electrode materials, and the like, and are the mainstream technology in the current electrochemical energy storage field.
Compared with other batteries made of positive electrode materials, the lithium iron phosphate battery (LiFePO 4, LFP) has the advantages of high safety, high stability, low cost, rich resources, long cycle life and the like. However, due to the limitations of the self crystal structure, poor conductivity, slow ion migration rate and the like, the improvement of the electrochemical performance of the material is greatly limited, and particularly, the problem of low rate performance is easily caused, so that the further development of the material in the future commercialization is influenced.
Generally, low rate performance represents slow lithium ion migration, and in order to solve the problem, researchers shorten the diffusion path of Li + by controlling the microstructure and size of LFP, but too small LFP crystallite size increases the polaron phenomenon of the structure to cause conductivity reduction, so that the rate performance of LFP is not good. Another effective way to do this is to develop porous lithium iron phosphate materials that utilize porous channels to provide fast transport channels for electrons and ions, and that both increase specific surface area and nano-scale pore wall thickness promote charge transfer and increase the diffusion rate of lithium ions. For example, CN115986065A discloses a method for preparing a lithium iron phosphate positive electrode material by a microwave-assisted hydrothermal method, a porous lithium iron phosphate precursor is prepared by a microwave-assisted hydrothermal method, and then sintered into carbon-coated porous lithium iron phosphate.
However, when lithium iron phosphate is manufactured into porous lithium iron phosphate, the porous lithium iron phosphate is easy to cause that the coating layer is dropped due to the possibility of cracking and breaking in the process of rolling the pole piece, and the porous lithium iron phosphate is directly contacted with electrolyte to accelerate the loss of the positive electrode active material, so that the stability of the battery is reduced, the capacity is reduced, and the cycle performance is accelerated to decay.
Therefore, a new strategy is needed to be adopted, and on the premise of maintaining a porous structure, the overall structural stability of the positive electrode material is improved, so that the lithium ion migration rate can be accelerated, the rate performance is improved, and the cracking problem in the process of pressing the pole piece can be avoided.
Disclosure of Invention
The following is a summary of the subject matter described in detail herein. This summary is not intended to limit the scope of the claims.
In view of the problems existing in the prior art, an object of the present disclosure is to provide a lithium iron phosphate composite material, and a preparation method and application thereof, wherein the preparation method comprises mixing porous inorganic nanofiber aerogel, a lithium source, an iron source and a phosphorus source to obtain a dispersion, performing spray drying to obtain a precursor, and sintering to obtain the lithium iron phosphate composite material. According to the method, the porous inorganic nanofiber aerogel is used for forming cladding on lithium iron phosphate in situ during synthesis of the lithium iron phosphate, the porous nanofiber is used for enabling lithium iron phosphate particles to be distributed more uniformly and not to be agglomerated any more, the double effects of the porous nanofiber and the aerogel can effectively shorten the transmission path of Li + and effectively improve the multiplying power performance of the obtained material, meanwhile, the supporting effect is achieved, damage caused by the processing processes such as pressing is avoided, the volume change of the obtained material during charging and discharging is relieved, the problems such as cracking are avoided, and the stability of the material is improved.
To achieve the purpose, the present disclosure adopts the following technical scheme:
In a first aspect, the present disclosure provides a method of preparing a lithium iron phosphate composite material, the method comprising:
Mixing porous inorganic nanofiber aerogel, a lithium source, an iron source, a phosphorus source and a carbon source to obtain a dispersion liquid, performing spray drying to obtain a precursor, and sintering to obtain the lithium iron phosphate composite material.
According to the method, the inorganic nanofiber aerogel is mixed in the raw materials of the lithium iron phosphate cathode material, so that a uniformly mixed precursor is obtained, and then, in the process of forming the lithium iron phosphate composite material, the porous inorganic nanofibers are positioned between lithium iron phosphate particles and on the surface of the lithium iron phosphate particles to form a certain coating layer, and in the whole, the lithium iron phosphate particles are attached to a porous skeleton built by the porous inorganic nanofibers, and the porous skeleton is supported by the nanofibers with a certain length-diameter ratio, so that the lithium iron phosphate composite material still has support and buffer after being stressed in the pressing process, and further, the cracking problem in the pressing process is avoided. In addition, the preparation method effectively increases the specific surface area of the positive electrode material on the premise of not influencing the structure of the positive electrode material, is beneficial to enhancing the contact with electrolyte and provides more electrochemical reaction active sites. The existence of the porous nano fiber enables the particle distribution of the anode material to be more uniform and not agglomerated any more, and the double effects of the porous nano fiber and the aerogel can effectively shorten the transmission path of Li +.
The characteristics of the aerogel with ultra-light and high elasticity can buffer the volume change brought by the charge and discharge of the lithium battery, and the nanofiber plays a supporting role in the lithium iron phosphate, so that the cracking condition of the pole piece during pressing can be avoided. The structure of the porous titanium dioxide nanofiber can be regulated and controlled by combining pore formers with different percentages by mass and electrostatic spinning parameters, so that more selectivity is provided for the subsequent composite anode material.
The following is an optional technical scheme of the present disclosure, but not a limitation of the technical scheme provided by the present disclosure, and the technical purpose and beneficial effect of the present disclosure can be better achieved and achieved by the following technical scheme.
As an alternative technical solution of the present disclosure, the method for preparing the porous inorganic nanofiber aerogel includes:
Mixing porous inorganic fiber and gel, and drying to obtain porous inorganic nanofiber aerogel.
The mixing of the porous inorganic fibers and the gelling agent can be performed in water and/or ethanol and other solvents to achieve sufficient and stable dispersion of the porous inorganic fibers, and then drying.
In one embodiment, the mass ratio of the porous inorganic nanofiber to the gelling agent is 1 (3-7), for example, 1:3, 1:3.5, 1:4, 1:4.5, 1:5, 1:5.5, 1:6, 1:6.5, or 1:7, etc., but not limited to the recited values, and other non-recited values within the above-recited values are equally applicable.
In one embodiment, the porous inorganic nanofiber is mixed with the gel in water in an amount of 6 to 12 times, for example, 6 times, 7 times, 8 times, 9 times, 10 times, 11 times, 12 times, etc., the total mass of other raw materials, but the present invention is not limited to the recited values, and other non-recited values within the above-mentioned range are equally applicable.
In one embodiment, the porous inorganic nanofibers comprise any one or a combination of at least two of titanium dioxide, silicon dioxide, or boron nitride, typical but non-limiting examples of which include titanium dioxide in combination with silicon dioxide, titanium dioxide in combination with boron nitride, or silicon dioxide in combination with boron nitride, further optionally porous silica nanofibers.
In one embodiment, the gelling agent comprises a silica sol.
The present disclosure selects the silica pair sol as a gel agent, which has good hydrophilicity, can be diluted to any concentration, and does not decrease stability.
In one embodiment, the gelling agent further comprises a coagulant.
In one embodiment, the coagulation promoting substance comprises an ester substance and/or an alcohol substance, wherein the ester substance comprises at least one of dibutyl carbonate, diethyl carbonate, ethyl acetate, methyl orthosilicate, ethyl orthosilicate, triethyl phosphate or tetraethyl orthosilicate, and further optionally ethyl orthosilicate, and the alcohol substance comprises at least one of methanol, ethanol or polyethylene glycol.
In one embodiment, the porous inorganic nanofiber aerogel further comprises a carbon material.
The present disclosure further dopes carbon materials in the porous inorganic nanofiber aerogel, which can improve the conductivity of the positive electrode material.
The method for preparing the carbon material doped porous titanium dioxide nanofiber aerogel comprises the steps of mixing porous titanium dioxide nanofiber, carbon material and gel, and drying to obtain the carbon material doped porous titanium dioxide nanofiber aerogel.
In one embodiment, the carbon material comprises graphene.
According to the method, the carbon material, particularly graphene, is introduced into the aerogel to dope, the carbon material and the inorganic nano fiber are utilized to form the composite material for the lithium iron phosphate, the conductivity of the carbon material can be improved in the preparation of the lithium iron phosphate positive electrode material, and a part of carbon sources for synthesizing the lithium iron phosphate can be replaced, so that the manufacturing cost is reduced, and the carbon material and the titanium dioxide nano fiber are in a uniformly dispersed and mixed state in the formed aerogel. In addition to graphene, other carbon materials such as carbon nanotubes may also be suitable. The reason for further selecting graphene is that the conductivity of the graphene is better in all carbon materials, the mixed contact area of the two-dimensional planar structure and titanium dioxide is larger, and the optimization effect is best.
In one embodiment, the carbon material comprises 0.01% -5% of the total mass of the porous inorganic nanofiber aerogel, for example, 0.01%, 0.05%, 0.1%, 0.5%, 0.8%, 1%, 1.3%, 1.5%, 1.8%, 2%, 2.3%, 2.5%, 2.8%, 3%, 3.3%, 3.5%, 3.8%, 4%, 4.3%, 4.5%, 4.8% or 5%, etc., but is not limited to the recited values, and other non-recited values within the above ranges are equally applicable.
In one embodiment, the method of drying comprises any one or a combination of at least two of freeze drying, supercritical drying, vacuum drying, or microwave drying, examples of which include a combination of freeze drying and supercritical drying, a combination of freeze drying and vacuum drying, a combination of freeze drying and microwave drying, a combination of supercritical drying and vacuum drying, or a combination of microwave drying and vacuum drying.
As an alternative technical solution of the present disclosure, the method for preparing the porous titania nanofiber includes:
mixing a titanium source, a pore-forming agent and a solvent to obtain a precursor solution, carrying out electrostatic spinning to obtain a spinning material, and calcining to obtain the porous titanium dioxide nanofiber.
In one embodiment, the pore former comprises camphene.
The method further selects camphene as a pore-forming agent, and the camphene and a titanium source can be simultaneously and stably present and do not react with each other, so that camphene can be pyrolyzed and volatilized at a temperature above 160 ℃, the volatilization temperature is lower, and the camphene can be sublimated from a solid phase directly, so that the pore-forming function can be realized at a lower temperature.
In one embodiment, the pore-forming agent is used in an amount of 0.1% -20% by mass of the titanium source, for example, 0.1%, 0.5%, 0.8%, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19% or 20%, etc., but not limited to the recited values, and other non-recited values within the above-recited ranges are equally applicable.
In one embodiment, the solid-to-liquid ratio of the titanium source to the solvent is 1g (2-5) mL, for example, 1g:2mL, 1g:2.3mL, 1g:2.6mL, 1g:2.9mL, 1g:3.2mL, 1g:3.5mL, 1g:3.8mL, 1g:4.1mL, 1g:4.4mL, 1g:4.7mL, or 1g:5mL, etc., but is not limited to the recited values, and other non-recited values within the above ranges are equally applicable.
In one embodiment, the solvent comprises ethanol and/or acetic acid.
In one embodiment, the solvent is ethanol and acetic acid in a volume ratio of (2-5): 1, for example, 2:1, 2.3:1, 2.5:1, 2.8:1, 3:1, 3.2:1, 3.5:1, 3.7:1, 4:1, 4.2:1, 4.5:1, 4.8:1, or 5:1, etc., but not limited to the recited values, other non-recited values in the above range are equally applicable.
In one embodiment, the resulting spun yarn is first dried at 160-180 ℃, e.g., 160 ℃, 162 ℃, 164 ℃, 166 ℃, 168 ℃, 170 ℃, 172 ℃, 174 ℃, 176 ℃, 178 ℃, 180 ℃, or the like, for a period of 10-24 hours, e.g., 10 hours, 12 hours, 14 hours, 16 hours, 18 hours, 20 hours, 22 hours, or 24 hours, and then calcined, although not limited to the recited values, other non-recited values within the above ranges are equally applicable.
The spinning material is firstly dried at 160-180 ℃, so that the pore-forming agent camphene can fully play a pore-forming role, and all pore-forming agents are volatilized and removed as much as possible.
As an alternative technical scheme of the disclosure, the voltage applied by the electrostatic spinning is 6-10 kV, for example, 6kV, 6.5V, 7kV, 7.5kV, 8kV, 8.5kV, 9kV, 9.5kV or 10kV, etc., the rotation speed is 30-80 rpm, for example, 30rpm, 40rpm, 50rpm, 60rpm, 70rpm or 80rpm, etc., the distance between the collecting plate and the needle is 8-25 cm, for example, 8cm, 10cm, 12cm, 14cm, 16cm, 18cm, 20cm, 23cm or 25cm, etc., but the electrostatic spinning is not limited to the listed values, and other values not listed in the above numerical range are equally applicable.
As an alternative solution of the present disclosure, the calcination is performed in an oxygen-containing atmosphere, and the calcination temperature is 300 to 650 ℃, such as 300 ℃, 330 ℃, 360 ℃, 390 ℃, 420 ℃, 450 ℃, 480 ℃, 510 ℃, 540 ℃, 570 ℃, 600 ℃, 630 ℃, 650 ℃ or the like, and the time is 2 to 5 hours, such as 2 hours, 2.5 hours, 3 hours, 3.5 hours, 4 hours, 4.5 hours, 5 hours or the like, but not limited to the recited values, and other non-recited values in the above numerical ranges are equally applicable.
In one embodiment, the process of preparing the porous titania nanofiber is performed in an environment with 20% -80% humidity.
As an alternative aspect of the present disclosure, the lithium source includes any one or a combination of at least two of lithium carbonate, lithium hydroxide, or lithium acetate, and typical but non-limiting examples of the combination include a combination of lithium carbonate and lithium hydroxide, a combination of lithium carbonate and lithium acetate, or a combination of lithium hydroxide and lithium acetate.
In one embodiment, the phosphorus source comprises monoammonium phosphate.
In one embodiment, the iron source comprises any one or a combination of at least two of iron phosphate tetrahydrate, iron oxide, iron sulfate, or iron oxide, typical but non-limiting examples of which include a combination of iron phosphate tetrahydrate and iron oxide, a combination of iron oxide and iron sulfate, a combination of iron oxide and iron phosphate tetrahydrate, a combination of iron oxide and iron oxide tetrahydrate, a combination of iron phosphate tetrahydrate and iron sulfate, or a combination of iron oxide and iron sulfate.
In one embodiment, the carbon source comprises any one or a combination of at least two of glucose, sucrose, starch, phenolic resin, dextrin, citric acid, oxalic acid, cellulose, or vitamins, typical but non-limiting examples of which include a combination of glucose and sucrose, a combination of glucose and starch, a combination of glucose and phenolic resin, a combination of glucose and dextrin, a combination of glucose and citric acid, a combination of glucose and oxalic acid, a combination of glucose and cellulose, a combination of glucose and vitamins, a combination of sucrose and starch, a combination of phenolic resin and dextrin, a combination of citric acid and oxalic acid, or a combination of cellulose and vitamins.
In one embodiment, the gas temperature of the spray drying is 160 to 300 ℃, for example 160 ℃, 180 ℃, 200 ℃, 220 ℃, 240 ℃, 260 ℃, 280 ℃, 300 ℃, etc., but is not limited to the recited values, and other non-recited values within the above-mentioned range are equally applicable.
In one embodiment, the gas comprises air and/or an inert gas, such as nitrogen, further optionally hot air.
The spray drying method has the advantages that the granulating function can be realized while drying is performed, the instant drying effect is ensured, and the size of particles can be controlled by regulating and controlling parameters.
In one embodiment, the sintering temperature is 400-700 ℃, such as 400 ℃, 430 ℃, 450 ℃, 480 ℃, 500 ℃, 520 ℃, 550 ℃, 570 ℃, 600 ℃, 620 ℃, 660 ℃, 680 ℃, 700 ℃ or the like, and the sintering time is 6-18 hours, such as 6 hours, 7 hours, 8 hours, 9 hours, 10 hours, 11 hours, 12 hours, 13 hours, 14 hours, 15 hours, 16 hours, 17 hours, 18 hours or the like, but not limited to the recited values, and other non-recited values within the above range are equally applicable.
In one embodiment, the amount of iron source and phosphorus source is controlled to be 1:1 molar ratio of iron element to phosphate.
In one embodiment, the amount of the porous inorganic nanofiber aerogel is controlled to be, for example, 0.03:1, 0.04:1, 0.05:1, 0.06:1, 0.07:1, or 0.08:1, etc., according to the molar ratio of the porous inorganic nanofiber to the iron element of (0.03-0.08): 1, but not limited to the recited values, and other non-recited values within the above-recited ranges are equally applicable.
In one embodiment, the amount of the lithium source is controlled to be 1:1, 1.01:1, 1.015:1, 1.02:1, 1.025:1 or 1.03:1 according to the molar ratio of the lithium element to the iron element of (1 to 1.03): 1, but the present invention is not limited to the above-mentioned values, and other non-mentioned values within the above-mentioned ranges are applicable.
In one embodiment, the amount of the carbon source is controlled to be 0.05:1, 0.06:1, 0.07:1, 0.08:1, 0.09:1, 0.10:1, 0.11:1, or 0.12:1, etc., according to the molar ratio of the carbon element to the iron element of (0.05-0.12): 1, but the present invention is not limited to the above-mentioned values, and other non-mentioned values in the above-mentioned value ranges are equally applicable.
As an optional technical scheme of the disclosure, the preparation method includes:
Mixing a titanium source, a pore-forming agent and a solvent, wherein the solid-to-liquid ratio of the titanium source to the solvent is controlled to be 1g (2-5) mL, the pore-forming agent comprises camphene, the consumption of the pore-forming agent accounts for 0.1-20% of the mass of the titanium source, the solvent is ethanol and acetic acid with the volume ratio of (2-5) being 1 to obtain a precursor liquid, the applied voltage is set to be 6-10 kV, the rotating speed is 30-80 rpm, the distance between a collecting plate and a needle head is 8-25 cm, electrostatic spinning is carried out on the obtained precursor liquid to obtain a spinning material, the obtained spinning material is dried for 10-24 h at 160-180 ℃, and the obtained spinning material is calcined for 2-5 h at 300-650 ℃ in an oxygen-containing atmosphere to obtain the porous titanium dioxide nanofiber;
Mixing porous titanium dioxide nanofiber, a carbon material and a gel agent in water, wherein the mass ratio of the porous inorganic nanofiber to the gel agent is 1 (3-7), the carbon material comprises graphene, the dosage of the carbon material accounts for 0.01% -5% of the mass of the porous titanium dioxide nanofiber aerogel, the gel agent comprises silica sol and/or a coagulation promoting substance, the dosage of the water accounts for 6-12 times of the total mass of other raw materials, and drying to obtain the carbon material doped porous titanium dioxide nanofiber aerogel;
The preparation method comprises the steps of mixing all raw materials according to the proportion of (0.03-0.08) of the molar quantity of Ti element in carbon-doped porous titanium dioxide nanofiber aerogel, the molar quantity of Li element in a lithium source, the molar quantity of Fe element in an iron source, the molar quantity of phosphate radical in a phosphorus source and the total molar quantity of carbon atoms in all raw materials, wherein (1-1.03) is 1:1 (0.05-0.12), mixing all raw materials, the lithium source comprises any one or a combination of at least two of lithium carbonate, lithium hydroxide and lithium acetate, the phosphorus source comprises monoammonium phosphate, the iron source comprises any one or a combination of at least two of iron tetrahydrate, ferric oxide, ferric sulfate and ferric oxide, the carbon source comprises any one or a combination of at least two of glucose, sucrose, starch, phenolic resin, dextrin, citric acid, oxalic acid, cellulose and vitamin, performing spray drying, performing hot air at 160-300 ℃ to obtain a precursor, and sintering at 400-700 ℃ to obtain the lithium phosphate composite material.
In a second aspect, the present disclosure provides a lithium iron phosphate composite material obtained according to the preparation method of the first aspect.
In a third aspect, the present disclosure provides a battery comprising the lithium iron phosphate composite of the second aspect.
Compared with the prior art, the method has the following advantages:
The method comprises the steps of compounding a precursor of a lithium iron phosphate positive electrode material by adopting porous inorganic nanofiber aerogel, so as to obtain a lithium iron phosphate composite material. The preparation method effectively increases the specific surface area of the positive electrode material on the premise of not influencing the structure of the positive electrode material, is beneficial to enhancing the contact with electrolyte and provides more electrochemical reaction active sites. The existence of the nano fibers enables the particles of the anode material to be distributed more uniformly and not agglomerated any more, and the double effects of the porous fiber and the aerogel can effectively shorten the transmission path of Li +;
The characteristics of the aerogel with ultra-light and high elasticity can buffer the volume change brought by the charge and discharge of the lithium battery, and the nanofiber plays a supporting role in the lithium iron phosphate, so that the cracking condition of the pole piece during pressing can be avoided. The structure of the porous inorganic nanofiber can be regulated and controlled by combining pore-forming agents with different percentage mass numbers and electrostatic spinning parameters, so that more selectivity is provided for the subsequent composite anode material.
According to the method, the carbon material, particularly graphene, is introduced into the aerogel to dope, and the carbon material and the inorganic nano fiber are utilized to form composite coating on the lithium iron phosphate, so that the conductivity of the carbon material can be improved, and a part of carbon sources for synthesizing the lithium iron phosphate can be replaced in the preparation of the lithium iron phosphate anode material, so that the manufacturing cost is reduced.
Other aspects will become apparent upon reading and understanding the accompanying drawings and detailed description.
Drawings
The accompanying drawings are included to provide a further understanding of the technology herein, and are incorporated in and constitute a part of this specification, illustrate technology herein and together with the description serve to explain, without limitation, the technology herein.
Fig. 1 is an SEM image of the lithium iron phosphate composite material obtained in example 4.
Detailed Description
The technical scheme of the present disclosure is further described below by means of specific embodiments.
It should be apparent to those skilled in the art that the examples are merely provided to aid in the understanding of the present disclosure and should not be construed as a specific limitation on the present disclosure.
Example 1
The embodiment provides a preparation method of a lithium iron phosphate composite material, which comprises the following steps:
(1) Uniformly mixing tetrabutyl titanate, glacial acetic acid and absolute ethyl alcohol in a ratio of 1:1:3, adding camphene with the content of the tetrabutyl titanate being 100% and the percentage by mass being 9%, uniformly mixing to form transparent light yellow liquid, and stirring overnight;
(2) Preparing a titanium dioxide nanofiber spinning material by adopting an electrostatic spinning method, namely, keeping the rotation speed of the solution in the step (1) at 40rpm at the applied voltage of 8kV, drying at 160 ℃ for 15 hours to remove the polymer, and then calcining and annealing at 400 ℃ for 3 hours to form porous titanium dioxide nanofiber;
(3) Adding the prepared porous titanium dioxide nanofiber and graphene with the mass fraction ratio of 1% into deionized water together for ultrasonic dispersion, then adding a gel agent for mixing, wherein the gel agent comprises silica sol and dibutyl carbonate, controlling the mass ratio of the porous titanium dioxide nanofiber to the deionized water to the gel agent to be 1:90:5, and freeze-drying to obtain graphene doped porous titanium dioxide nanofiber aerogel;
(4) Preparing dispersion liquid from raw materials of lithium carbonate, ferric phosphate and carbon source glucose of the graphene doped porous titanium dioxide nanofiber aerogel and a positive electrode material, uniformly dispersing and mixing materials in water according to the molar ratio of titanium, lithium, iron and carbon elements of 0.05:1.01:1:0.08, setting the spray drying temperature to be 210 ℃, and performing spray drying to obtain a precursor;
(5) And (3) sintering the mixed substance obtained in the step (4) at a high temperature of 650 ℃ for 8 hours to obtain the graphene doped porous titanium dioxide nanofiber aerogel composite coated lithium iron phosphate material.
Example 2
The present example provides a method for preparing a lithium iron phosphate composite material, in which the amount of camphene used in step (1) is adjusted from 6% to 9%, and the other conditions are exactly the same as in example 1 except for the above.
Example 3
The present embodiment provides a method for preparing a lithium iron phosphate composite material, in which the amount of camphene is adjusted from 6% to 9% in step (1), the amount of graphene is adjusted from 1% to 3% in step (3), and the sintering time is adjusted from 8 hours to 10 hours in step (5), except for the above, the other conditions are exactly the same as in embodiment 1.
Example 4
The present embodiment provides a method for preparing a lithium iron phosphate composite material, in which the amount of camphene is adjusted from 6% to 12% in step (1), the amount of graphene is adjusted from 1% to 3% in step (3), and the sintering time is adjusted from 8 hours to 10 hours in step (5), except for the above, the other conditions are exactly the same as in embodiment 1.
Example 5
The present example provides a method for preparing a lithium iron phosphate composite material, in which the amount of camphene is adjusted from 6% to 12% in step (1), the temperature of calcination is adjusted to 500 ℃ in step (2), the amount of graphene is adjusted from 1% to 3% in step (3), and the sintering time is adjusted from 8 hours to 10 hours in step (5), except for the above, the other conditions are exactly the same as in example 1.
Example 6
The present embodiment provides a method for preparing a lithium iron phosphate composite material, which does not use graphene in step (3), and the other conditions are exactly the same as those of embodiment 4 except for the above.
Example 7
The present embodiment provides a method for preparing a lithium iron phosphate composite material, in which carbon nanotubes are used instead of graphene in step (3), and the other conditions are exactly the same as in embodiment 4 except for the above.
Example 8
The present example provides a method for preparing a lithium iron phosphate composite material, in which the amount of camphene is adjusted from 12% to 1% in step (1), and the other conditions are exactly the same as in example 4 except for the above.
Example 9
The present example provides a method for preparing a lithium iron phosphate composite material, in which the amount of camphene is adjusted from 12% to 3% in step (1), and the other conditions are exactly the same as in example 4 except for the above.
Example 10
The present example provides a method for preparing a lithium iron phosphate composite material, in which the amount of camphene is adjusted from 12% to 20% in step (1), and the other conditions are exactly the same as in example 4 except for the above.
Example 11
The present example provides a method for preparing a lithium iron phosphate composite material, in which the amount of camphene is adjusted from 12% to 23% in step (1), and the conditions are exactly the same as in example 4 except for the above.
Example 12
The present embodiment provides a method for preparing a lithium iron phosphate composite material, in which the amount of graphene is adjusted from 3% to 0.5% in step (3), and the sintering time is adjusted from 8h to 10h in step (5), and the other conditions are exactly the same as in embodiment 1 except for the above.
Example 13
The present embodiment provides a method for preparing a lithium iron phosphate composite material, in which the amount of graphene is adjusted from 3% to 5.5% in step (3), and the sintering time is adjusted from 8h to 10h in step (5), and the other conditions are exactly the same as in embodiment 1 except for the above.
Comparative example 1
The comparative example provides a preparation method of a lithium iron phosphate composite material, wherein the preparation method does not use porous titanium dioxide nanofiber aerogel, and the preparation method comprises the following steps:
the lithium source, the phosphorus source, the iron source and the carbon source in the step (4) of example 4 were prepared into a dispersion, and spray-dried, and sintered at 650 ℃ for 10 hours to obtain a lithium iron phosphate composite material.
Comparative example 2
This comparative example provides a method for preparing lithium iron phosphate composite material, which does not use camphene in step (1), and the other conditions are exactly the same as in example 4 except for the above.
Comparative example 3
This comparative example provides a method for preparing a lithium iron oxide composite material by mixing only porous titania nanofibers and graphene without using a gelling agent in step (3) and freeze-drying, and applying the obtained sample to step (4), except for the above, the other conditions are exactly the same as in example 4.
Control group 1
A method for preparing a lithium iron phosphate positive electrode material disclosed by CN115986065A comprises the following steps:
(1) Mixing lithium acetate dihydrate, ferrous sulfate heptahydrate and phosphoric acid according to a molar ratio of 1:1:1, and placing the mixture in the lithium acetate dihydrate and pure water (1:25) for uniform mixing;
(2) Adding polyethylene glycol with the mass of 0.004 times of the precursor solution and glucose with the mass of 0.02 times of the precursor solution into the precursor solution, placing the mixture into a microwave reaction kettle, and controlling the microwave power to be 60W, the microwave frequency to be 1000MHz and the temperature to be 180 ℃ for reaction for 40min;
(3) Cooling to room temperature, centrifugally separating to obtain solid, washing with pure water for 3-5 times, and drying at 90 ℃ for 6 hours to obtain a porous lithium iron phosphate precursor;
(4) And sintering the porous lithium iron phosphate precursor for 7 hours at 600 ℃ in a nitrogen atmosphere to prepare the carbon-coated porous lithium iron phosphate.
The materials or composite materials obtained in the above examples, comparative examples and control groups are used as positive electrode materials to prepare button cells for testing the electrochemical performance of lithium ion batteries, and the specific steps are as follows:
Uniformly mixing an anode material, a conductive agent acetylene black and an adhesive polyvinylidene fluoride into N-methyl pyrrolidone according to a ratio (8:1:1), coating the mixture on an aluminum foil, placing the aluminum foil in a vacuum drying oven at 120 ℃ for drying for 12 hours, assembling a battery in an argon glove box after drying, tabletting at 30MPa to obtain a circular sheet anode plate with the diameter of 1cm, wherein the cathode is a metal lithium sheet, the electrolyte is LiPF 6 -EC:DMC (volume ratio 1:1), and the polypropylene porous membrane is used as a diaphragm.
Table 1 shows the rate performance test of battery samples, the charge/discharge cut-off voltage was 2.7 to 4.3V, and the charge/discharge cycles were performed for 5 weeks at current densities of 0.2C,1C,3C,5C,8C, respectively. Table 2 shows the sample battery cycle performance test, the charge/discharge cut-off voltage is 2.7-4.3 v, and the current density is 1c=160 mA/g.
TABLE 1
TABLE 2
As can be seen from tables 1 and 2:
Table 1 shows the discharge capacities of different examples (0.2C, 1C,3C,5C, 8C) at different magnifications, and it can be seen from the table that the discharge capacities of example 4 at different magnifications are respectively 154.2mAh/g, 146.5mAh/g, 139.8mAh/g, 130.2mAh/g and 119.9mAh/g, which are the best ones in the discharge capacity performance of all examples, and the porous titanium dioxide nanofiber aerogel is introduced for compounding in the preparation of the positive electrode material to form the lithium iron phosphate with a nano porous structure, so that the lithium ion transmission path is shortened, and the material has excellent reversibility for lithium ion extraction and intercalation in the charge-discharge process, and can realize lithium ion intercalation even at high magnification. While cycle performance was also excellent compared to other examples and comparative examples, the cycle retention after 100 cycles of discharge at 1C was 96.1%. Fig. 1 is an SEM image of the lithium ion battery composite positive electrode material prepared in example 4, and after 5000 times magnification, primary particles of lithium iron phosphate and agglomerated secondary particles with uniform size scale can be seen, and the structure morphology is well dispersed uniformly, and only a small amount of agglomeration effect is achieved.
Comparison of examples 1-4 and examples 8-11 adjusts the amount of camphene, and it was found that the discharge capacity of the battery also exhibited a decrease when the amount of camphene was decreased at 0.2C and other rates, probably because too little camphene did not have a way to make enough porosity, and did not shorten the lithium ion diffusion channel to achieve efficient lithium ion transport. When the using amount of camphene is too high or exceeds a limit value, the cycle retention rates of the embodiment 10 and the embodiment 11 are 93.8% and 93.4% after 100 cycles, which is probably because the existence of too much pore-forming agent damages the structure of the nanofiber, the nanofiber has no supporting effect, the nanofiber is easy to crack when pressed by a pole piece, and positive lithium ions are continuously separated and embedded in the repeated charge and discharge process, the volume of the material expands and contracts, the possibility of cracking of the material is increased, and the cycle performance is reduced.
Comparing examples 1,3-4 and examples 12-13 adjusts the amount of graphene, and discovers that when the amount of graphene is too small, the discharge capacity of the battery is low, which may be caused by too low conductivity of the cathode material due to too small amount of graphene, which affects the electrical performance of the cathode material, and the discharge capacity is higher and higher along with the increase of graphene, but too much graphene may cause self-agglomeration together, which hinders the transmission of lithium ions.
Example 4, compared to comparative examples 1-3, the lithium iron phosphate was prepared in a normal manner without using titanium dioxide aerogel, and both rate performance and cycle performance were lower than example 4, demonstrating the desirability of the present disclosure. Compared with the embodiment 4, the performance of the composite lithium iron phosphate prepared by simply preparing the nanofiber aerogel without introducing camphene for pore-forming is slightly lower, and the performance of the composite lithium iron phosphate prepared by simply preparing the nanofiber aerogel is better than that of the composite lithium iron phosphate prepared by preparing the composite lithium iron phosphate prepared by simply preparing the nanofiber aerogel in the embodiment 1, and the improvement effect of the mode of introducing the aerogel on the electrical performance of the lithium iron phosphate is proved.
Claims (4)
1. A method for preparing a lithium iron phosphate composite material, the method comprising:
Mixing a titanium source, a pore-forming agent and a solvent, wherein the solid-to-liquid ratio of the titanium source to the solvent is controlled to be 1g (2-5) mL, the pore-forming agent comprises camphene, the consumption of the pore-forming agent accounts for 0.1-20% of the mass of the titanium source, the solvent is ethanol and acetic acid with the volume ratio of (2-5) being 1 to obtain a precursor liquid, the applied voltage is set to be 6-10 kV, the rotating speed is 30-80 rpm, the distance between a collecting plate and a needle head is 8-25 cm, electrostatic spinning is carried out on the obtained precursor liquid to obtain a spinning material, the obtained spinning material is dried for 10-24 h at 160-180 ℃, and the obtained spinning material is calcined for 2-5 h at 300-650 ℃ in an oxygen-containing atmosphere to obtain the porous titanium dioxide nanofiber;
Mixing porous titanium dioxide nanofiber, a carbon material and a gel in water, wherein the mass ratio of the porous titanium dioxide nanofiber to the gel is 1 (3-7), the gel comprises silica sol and/or a coagulation promoting substance, the water consumption is 6-12 times of the total mass of other raw materials, and the porous titanium dioxide nanofiber aerogel doped with the carbon material is obtained after drying, the carbon material comprises graphene, and the carbon material consumption accounts for 0.01-5% of the mass of the porous titanium dioxide nanofiber aerogel;
According to the molar quantity of Ti element in the carbon doped porous titanium dioxide nanofiber aerogel, the molar quantity of Li element in a lithium source, the molar quantity of Fe element in an iron source, the molar quantity of phosphate radical in a phosphorus source and the total molar quantity ratio of the carbon source to carbon atoms in all raw materials (0.03-0.08): 1:1:1 (0.05-0.12), mixing all raw materials, wherein the lithium source comprises any one or a combination of at least two of lithium carbonate, lithium hydroxide or lithium acetate, the phosphorus source comprises ammonium dihydrogen phosphate, the iron source comprises any one or a combination of at least two of iron tetrahydrate, ferric oxide, ferric sulfate or ferric oxide, the carbon source comprises any one or a combination of at least two of glucose, sucrose, starch, phenolic resin, dextrin, citric acid, oxalic acid, cellulose or vitamins, dispersing the above materials into a solvent to obtain a dispersion, spray drying the dispersion, using 160-300 ℃ of the dispersion, and performing heat sintering at the temperature of 400-18 ℃ to obtain the composite material.
2. The method of claim 1, wherein the procoagulant substance comprises an ester substance and/or an alcohol substance.
3. A lithium iron phosphate composite material, characterized in that it is obtained according to the preparation method of claim 1 or 2.
4. A battery comprising the lithium iron phosphate composite of claim 3.