CN110139005A - A kind of mobile phone camera eyeglass steel process - Google Patents

A kind of mobile phone camera eyeglass steel process Download PDF

Info

Publication number
CN110139005A
CN110139005A CN201910008111.XA CN201910008111A CN110139005A CN 110139005 A CN110139005 A CN 110139005A CN 201910008111 A CN201910008111 A CN 201910008111A CN 110139005 A CN110139005 A CN 110139005A
Authority
CN
China
Prior art keywords
glass substrate
mobile phone
phone camera
jig
camera eyeglass
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CN201910008111.XA
Other languages
Chinese (zh)
Inventor
张梓丰
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Dongguan Hong Han Electronic Materials Co Ltd
Original Assignee
Dongguan Hong Han Electronic Materials Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Dongguan Hong Han Electronic Materials Co Ltd filed Critical Dongguan Hong Han Electronic Materials Co Ltd
Priority to CN201910008111.XA priority Critical patent/CN110139005A/en
Publication of CN110139005A publication Critical patent/CN110139005A/en
Pending legal-status Critical Current

Abstract

The invention discloses a kind of mobile phone camera eyeglass steel process, include the following steps: to spray one layer of protection ink on the surface of glass baseplate;Glass baseplate is cut into 1.2 times of the glass substrate that volume is mobile phone camera eyeglass;Glass substrate is fixed on jig by UV glue;Jig is fixedly mounted on CNC machine, progress chamfering is sharp processing;The UV glue on jig is removed by impregnating;Glass substrate is inserted in insert rack;Ink retreating agent rinses glass substrate and carries out ink retreating;Glass substrate is placed in tempering in annealing furnace;Silk-screen processing is carried out to the edge of glass substrate;Glass substrate is placed with vacuum plating furnace, is electroplated;In lens surface bonding protective film, the processing of mobile phone camera eyeglass is completed.By the design of jig and insert rack, glass substrate is first placed on progress shape shaping on jig, the jig being laid out using square matrix is easy to implement the automation multiple groups processing of CNC machine.

Description

A kind of mobile phone camera eyeglass steel process
Technical field
The invention belongs to mobile phone camera eyeglass fields, more specifically more particularly to a kind of mobile phone camera eyeglass steel Chemical industry skill.
Background technique
The digital camera functionality of mobile phone refers to whether mobile phone can be clapped by built-in or external digital camera Static images or short-movie shooting are taken the photograph, as a new additional function of mobile phone, the digital camera functionality of mobile phone has been obtained rapidly Development.With the raising of camera pixel, shooting effect also becomes closer to traditional card camera even low side single-lens reflex camera phase Machine.Mobile phone camera be divided into it is built-in with it is external, built-in camera refer to camera in interior of mobile phone, it is more convenient.External mobile phone is logical It crosses data line or mobile phone lower interface is connected with digital camera, to complete all shooting functions of digital camera.External digital The advantages of camera, is that the weight of mobile phone can be mitigated, and external digital camera is light-weight, easy to carry, application method letter It is single.
The eyeglass of mobile phone camera is mounted on the camera of mobile phone back side, is had for protecting camera, while also Have anti-sticking, is not easy to be infected with the characteristic of fingerprint.However existing mobile phone camera eyeglass processing when, for glass baseplate Sharp processing when, glass substrate is not easy accurate fixation, and process velocity is slower, and common glass substrate is when being electroplated, It is not easy to manage in batches.It would therefore be desirable to propose a kind of mobile phone camera eyeglass steel process.
Summary of the invention
The purpose of the present invention is to solve disadvantages existing in the prior art, and a kind of mobile phone camera eyeglass proposed Steel process.
To achieve the above object, the invention provides the following technical scheme:
A kind of mobile phone camera eyeglass steel process, includes the following steps:
S1, sprayed protection ink spray one layer of protection ink on the surface of glass baseplate;
Glass baseplate is cut into 1.2 times of the glass substrate that volume is mobile phone camera eyeglass by S2, sawing sheet;
S3, pendulum, glass substrate is placed on jig;
Glass substrate is fixed on jig by S4, dispensing by UV glue;
Jig is fixedly mounted on CNC machine by S5, CNC chamfering, carries out chamfering as shape shaping processing;
S6, degumming remove the UV glue on jig in such a way that soak impregnates;
S7, insert rack, after the completion insert glass substrate in insert rack;
S8, ink retreating rinse glass substrate by ink retreating agent and carry out ink retreating;
S9, cleaning carry out side cleaning after ink retreating;
Glass substrate, is then placed in annealing furnace by S10, tempering, carries out tempering processing;
S11, cleaning, tempering carry out secondary cleaning after the completion;
S12, pad carry out a pad to glass substrate;
S13, silk-screen carry out silk-screen processing to the edge of glass substrate;
S14, pad carry out secondary pad after silk-screen processing;
Glass substrate is placed with vacuum plating furnace, is electroplated by S15, plating;
S16, pad complete pad three times after plating;
S17, pad pasting complete the processing of mobile phone camera eyeglass in lens surface bonding protective film after pad three times.
Preferably, the sprayed protection ink oil mentioned in the S1 is waterborne glass ink.
Preferably, the soak mentioned in the S6 is the mixed liquor of citric acid and water, the levels of the citric acid For 5-15%.
Preferably, the tempering time for the glass tempering mentioned in the S10 is 4.45-5H, and the furnace temperature of glass tempering furnace It is maintained at 405-415 DEG C.
Preferably, mentioned in the S5 on CNC machine carry out shaping processing when, need to carry out Multi-angle water spray drop simultaneously Temperature.
Preferably, the vacuum plating mentioned in the S15, by the way of ion source bombardment, high-temperature gasification plating.
Preferably, 4*5 totally 20 fixed salient points in length and breadth are provided on the jig mentioned in the S3.
Preferably, in the insert rack mentioned in the S7, be provided in length and breadth 4*5 totally 20 it is identical with glass substrate structure insert Slot.
Preferably, the glass substrate mentioned in the S2 with a thickness of 0.4-1.5mm.
Technical effect and advantage of the invention: a kind of mobile phone camera eyeglass steel process provided by the invention, by controlling Glass substrate is first placed on progress shape shaping on jig, the jig being laid out using square matrix, convenient for real by the design of tool and insert rack Existing CNC machine automation multiple groups processing;By the design of insert rack, is handled convenient for single multiple groups, be convenient for managing in batches, and mention High speed of production;And when carrying out vacuum plating, the design of insert rack is put into and takes out convenient for whole, one-side electroplating, whole matter Amount is more evenly.
Specific embodiment
In order to make the objectives, technical solutions, and advantages of the present invention clearer, below in conjunction with specific embodiment, to this Invention is further elaborated.It should be appreciated that the specific embodiments described herein are merely illustrative of the present invention, not For limiting the present invention.Based on the embodiments of the present invention, those of ordinary skill in the art are not before making creative work Every other embodiment obtained is put, shall fall within the protection scope of the present invention.
Embodiment 1
A kind of mobile phone camera eyeglass steel process, includes the following steps:
S1, sprayed protection ink spray one layer of protection ink on the surface of glass baseplate;The protection ink oil is aqueous glass Glass ink;
Glass baseplate is cut into 1.2 times of the glass substrate that volume is mobile phone camera eyeglass by S2, sawing sheet;Glass base Piece with a thickness of 0.4mm;
S3, pendulum, glass substrate is placed on jig;4*5 totally 20 fixed salient points in length and breadth are provided on jig;
Glass substrate is fixed on jig by S4, dispensing by UV glue, and glass substrate is fixed in fixed salient point;
Jig is fixedly mounted on CNC machine by S5, CNC chamfering, carries out chamfering as shape shaping processing;It is enterprising in CNC machine When row shaping is processed, need to carry out Multi-angle water spray cooling simultaneously;
S6, degumming remove the UV glue on jig in such a way that soak impregnates;Soak is the mixed of citric acid and water Liquid is closed, the levels of the citric acid are 5%;
S7, insert rack, after the completion insert glass substrate in insert rack;4*5 totally 20 and glass in length and breadth are provided in insert rack The identical slot of substrate structure;
S8, ink retreating rinse glass substrate by ink retreating agent and carry out ink retreating;
S9, cleaning carry out side cleaning after ink retreating;
Glass substrate, is then placed in annealing furnace by S10, tempering, carries out tempering processing;The tempering time of glass tempering 405 DEG C are maintained at for the furnace temperature of 4.45H, and glass tempering furnace;
S11, cleaning, tempering carry out secondary cleaning after the completion;
S12, pad carry out a pad to glass substrate;
S13, silk-screen carry out silk-screen processing to the edge of glass substrate;
S14, pad carry out secondary pad after silk-screen processing;
Glass substrate is placed with vacuum plating furnace, is electroplated by S15, plating;Vacuum plating is banged using ion source It hits, the mode of high-temperature gasification plating;
S16, pad complete pad three times after plating;
S17, pad pasting complete the processing of mobile phone camera eyeglass in lens surface bonding protective film after pad three times.
Embodiment 2
A kind of mobile phone camera eyeglass steel process, includes the following steps:
S1, sprayed protection ink spray one layer of protection ink on the surface of glass baseplate;The protection ink oil is aqueous glass Glass ink;
Glass baseplate is cut into 1.2 times of the glass substrate that volume is mobile phone camera eyeglass by S2, sawing sheet;Glass base Piece with a thickness of 1.0mm;
S3, pendulum, glass substrate is placed on jig;4*5 totally 20 fixed salient points in length and breadth are provided on jig;
Glass substrate is fixed on jig by S4, dispensing by UV glue, and glass substrate is fixed in fixed salient point;
Jig is fixedly mounted on CNC machine by S5, CNC chamfering, carries out chamfering as shape shaping processing;It is enterprising in CNC machine When row shaping is processed, need to carry out Multi-angle water spray cooling simultaneously;
S6, degumming remove the UV glue on jig in such a way that soak impregnates;Soak is the mixed of citric acid and water Liquid is closed, the levels of the citric acid are 10%;
S7, insert rack, after the completion insert glass substrate in insert rack;4*5 totally 20 and glass in length and breadth are provided in insert rack The identical slot of substrate structure;
S8, ink retreating rinse glass substrate by ink retreating agent and carry out ink retreating;
S9, cleaning carry out side cleaning after ink retreating;
Glass substrate, is then placed in annealing furnace by S10, tempering, carries out tempering processing;The tempering time of glass tempering 410 DEG C are maintained at for the furnace temperature of 4.8H, and glass tempering furnace;
S11, cleaning, tempering carry out secondary cleaning after the completion;
S12, pad carry out a pad to glass substrate;
S13, silk-screen carry out silk-screen processing to the edge of glass substrate;
S14, pad carry out secondary pad after silk-screen processing;
Glass substrate is placed with vacuum plating furnace, is electroplated by S15, plating;Vacuum plating is banged using ion source It hits, the mode of high-temperature gasification plating;
S16, pad complete pad three times after plating;
S17, pad pasting complete the processing of mobile phone camera eyeglass in lens surface bonding protective film after pad three times.
Embodiment 3
A kind of mobile phone camera eyeglass steel process, includes the following steps:
S1, sprayed protection ink spray one layer of protection ink on the surface of glass baseplate;The protection ink oil is aqueous glass Glass ink;
Glass baseplate is cut into 1.2 times of the glass substrate that volume is mobile phone camera eyeglass by S2, sawing sheet;Glass base Piece with a thickness of 1.5mm;
S3, pendulum, glass substrate is placed on jig;4*5 totally 20 fixed salient points in length and breadth are provided on jig;
Glass substrate is fixed on jig by S4, dispensing by UV glue, and glass substrate is fixed in fixed salient point;
Jig is fixedly mounted on CNC machine by S5, CNC chamfering, carries out chamfering as shape shaping processing;It is enterprising in CNC machine When row shaping is processed, need to carry out Multi-angle water spray cooling simultaneously;
S6, degumming remove the UV glue on jig in such a way that soak impregnates;Soak is the mixed of citric acid and water Liquid is closed, the levels of the citric acid are 15%;
S7, insert rack, after the completion insert glass substrate in insert rack;4*5 totally 20 and glass in length and breadth are provided in insert rack The identical slot of substrate structure;
S8, ink retreating rinse glass substrate by ink retreating agent and carry out ink retreating;
S9, cleaning carry out side cleaning after ink retreating;
Glass substrate, is then placed in annealing furnace by S10, tempering, carries out tempering processing;The tempering time of glass tempering 415 DEG C are maintained at for the furnace temperature of 5H, and glass tempering furnace;
S11, cleaning, tempering carry out secondary cleaning after the completion;
S12, pad carry out a pad to glass substrate;
S13, silk-screen carry out silk-screen processing to the edge of glass substrate;
S14, pad carry out secondary pad after silk-screen processing;
Glass substrate is placed with vacuum plating furnace, is electroplated by S15, plating;Vacuum plating is banged using ion source It hits, the mode of high-temperature gasification plating;
S16, pad complete pad three times after plating;
S17, pad pasting complete the processing of mobile phone camera eyeglass in lens surface bonding protective film after pad three times.
Three groups of embodiments specific data when implementing are as follows:
Embodiment 1 Embodiment 2 Embodiment 3
Glass substrate thickness 0.4mm 1.0mm 1.5mm
Citric acid concentration 5% 10% 15%
The tempering time 4.45H 4.8H 5.0H
Tempering temperature 405℃ 410℃ 415℃
When carrying out tempering production, the supplemental characteristic for needing to be arranged is arranged not glass for lenses according to the type of lenses of production Together, specific data are as follows:
In summary: a kind of mobile phone camera eyeglass steel process provided by the invention, by the design of jig and insert rack, Glass substrate is first placed on progress shape shaping on jig, it is more to be easy to implement the automation of CNC machine for the jig being laid out using square matrix Group processing;By the design of insert rack, is handled convenient for single multiple groups, be convenient for managing in batches, and improve speed of production;And When carrying out vacuum plating, the design of insert rack is put into and takes out convenient for whole, and one-side electroplating, total quality is more evenly.
Finally, it should be noted that the foregoing is only a preferred embodiment of the present invention, it is not intended to restrict the invention, Although the present invention is described in detail referring to the foregoing embodiments, for those skilled in the art, still may be used To modify the technical solutions described in the foregoing embodiments or equivalent replacement of some of the technical features, All within the spirits and principles of the present invention, any modification, equivalent replacement, improvement and so on should be included in of the invention Within protection scope.

Claims (9)

1. a kind of mobile phone camera eyeglass steel process, characterized by the following steps:
S1, sprayed protection ink spray one layer of protection ink on the surface of glass baseplate;
Glass baseplate is cut into 1.2 times of the glass substrate that volume is mobile phone camera eyeglass by S2, sawing sheet;
S3, pendulum, glass substrate is placed on jig;
Glass substrate is fixed on jig by S4, dispensing by UV glue;
Jig is fixedly mounted on CNC machine by S5, CNC chamfering, carries out chamfering as shape shaping processing;
S6, degumming remove the UV glue on jig in such a way that soak impregnates;
S7, insert rack, after the completion insert glass substrate in insert rack;
S8, ink retreating rinse glass substrate by ink retreating agent and carry out ink retreating;
S9, cleaning carry out side cleaning after ink retreating;
Glass substrate, is then placed in annealing furnace by S10, tempering, carries out tempering processing;
S11, cleaning, tempering carry out secondary cleaning (excusing from death wave, two processing solution tanks, spray, four Rinsing Areas) after the completion;
S12, pad carry out a pad to glass substrate;
S13, silk-screen carry out silk-screen processing to the edge of glass substrate;
S14, pad carry out secondary pad after silk-screen processing;
Glass substrate is placed with vacuum plating furnace, is electroplated by S15, plating;
S16, pad complete pad three times after plating;
S17, pad pasting complete the processing of mobile phone camera eyeglass in lens surface bonding protective film after pad three times.
2. a kind of mobile phone camera eyeglass steel process according to claim 1, it is characterised in that: mentioned in the S1 Sprayed protection ink oil is waterborne glass ink.
3. a kind of mobile phone camera eyeglass steel process according to claim 1, it is characterised in that:, it is mentioned in the S6 Soak be citric acid and water mixed liquor, the levels of the citric acid are 5-15%.
4. a kind of mobile phone camera eyeglass steel process according to claim 1, it is characterised in that: mentioned in the S10 Tempering time of glass tempering be 4.45-5H, and the furnace temperature of glass tempering furnace is maintained at 405-415 DEG C.
5. a kind of mobile phone camera eyeglass steel process according to claim 1, it is characterised in that: mentioned in the S5 When carrying out shaping processing on CNC machine, need to carry out Multi-angle water spray cooling simultaneously.
6. a kind of mobile phone camera eyeglass steel process according to claim 1, it is characterised in that: mentioned in the S15 Vacuum plating, using ion source bombardment, high-temperature gasification plating by the way of.
7. a kind of mobile phone camera eyeglass steel process according to claim 1, it is characterised in that: mentioned in the S3 4*5 totally 20 fixed salient points in length and breadth are provided on jig.
8. a kind of mobile phone camera eyeglass steel process according to claim 1, it is characterised in that: mentioned in the S7 In insert rack, it is provided with 4*5 totally 20 slots identical with glass substrate structure in length and breadth.
9. a kind of mobile phone camera eyeglass steel process according to claim 1, it is characterised in that: mentioned in the S2 Glass substrate with a thickness of 0.4-1.5mm.
CN201910008111.XA 2019-01-04 2019-01-04 A kind of mobile phone camera eyeglass steel process Pending CN110139005A (en)