CN109399948A - A kind of electric slide-mouse glass-making processes - Google Patents

A kind of electric slide-mouse glass-making processes Download PDF

Info

Publication number
CN109399948A
CN109399948A CN201811384789.XA CN201811384789A CN109399948A CN 109399948 A CN109399948 A CN 109399948A CN 201811384789 A CN201811384789 A CN 201811384789A CN 109399948 A CN109399948 A CN 109399948A
Authority
CN
China
Prior art keywords
glass
printing
ink
original sheet
silk
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
CN201811384789.XA
Other languages
Chinese (zh)
Other versions
CN109399948B (en
Inventor
云猛
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Chongqing Siyuxing Electronic Materials Co Ltd
Original Assignee
Chongqing Siyuxing Electronic Materials Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Chongqing Siyuxing Electronic Materials Co Ltd filed Critical Chongqing Siyuxing Electronic Materials Co Ltd
Priority to CN201811384789.XA priority Critical patent/CN109399948B/en
Publication of CN109399948A publication Critical patent/CN109399948A/en
Application granted granted Critical
Publication of CN109399948B publication Critical patent/CN109399948B/en
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

The invention discloses a kind of electric slide-mouse glass-making processes, including frosting, polishing, silk-screen printing, solve the problems, such as the semi-transparent place's color color difference of slide-mouse glass traditional handicraft, switch between the numeric keypad when full page color made and lighting more naturally, visual effect greatly promotes.

Description

A kind of electric slide-mouse glass-making processes
Technical field
The present invention relates to laptop slide-mouse production technical fields, and in particular to a kind of electric slide-mouse glass manufacture side Method.
Background technique
The electric slide-mouse of pen, i.e. laptop slide-mouse are located at middle part, common shape in front of keyboard of notebook computer and are generally One small rectangular replaces mouse operation and control computer for finger touch.
Mat glass is widely used in the touch-controls such as mobile phone, computer field.To the processing method of this product, traditional way is It is made into single side frosted with physics sandblasting, then is fabricated to the size of client's required product and color fits in touchpad surface.
For pen electricity slide-mouse glass, according to the actual situation, the symbols such as press figure key on glass is needed, that is, form number Keyboard.Traditional handicraft prints the semi-transparent oil of IR by the way of hollowed printing at the numeric keypad for needing to present semi-transparent lighting effects Ink.The pen electricity slide-mouse produced using traditional approach is since shielding is poor, visible light source after polishing, and semi-transparent area and whole color difference regard Feel obvious, visual effect is poor.
Summary of the invention
In view of this, the purpose of the present invention is to provide a kind of electric slide-mouse glass-making processes.
In order to achieve the above objectives, the invention provides the following technical scheme:
The present invention a kind of electric slide-mouse glass-making processes, comprising the following steps: S1. does a surface of original sheet glass close Envelope processing, original sheet glass it is another surface exposed.
S2. the surface exposed using pretreatment fluid cleaning original sheet glass, pretreatment fluid includes with weight at assignment system
Measure the sulfuric acid of 10%-15%, 5%-10% that proportion calculates hydrofluoric acid, remaining be water.
S3. the original sheet glass handled is put into frosting chemical pond and carries out frosting etching process, standing time is
1-3 minutes, the configuration of the ingredient of frosting liquor include the 40% hydrogen fluoride ammonia calculated with weight proportion,
10% barium sulfate, 20% sulfuric acid, remaining is water.
S4. the original sheet glass after frosting is rinsed with water completely, is put into chemical polishing solution and carries out attenuated polishing,
Standing time is -5 minutes 1 minute, and the ingredient configuration of chemical polishing solution includes in terms of weight proportion
The hydrofluoric acid of the 60%-70% of calculation, remaining is water.
S5. the original sheet glass after polishing is removed into sealing, rinsed well.
S6. silk-screen ink prints: silk-screen screen frame being located on printing machine platform, printing apparatus positioning is placed in
On board and fixed, bright by original sheet glass is put into jig up, is repeatedly printed with ink;
S7. the glass after the completion of silk-screen is put into oven and is toasted, baking temperature is 150 degrees Celsius, when baking
Between be 10-15 minutes.
Further, in the S1, the mode of encapsulation process are as follows: the original sheet glass that need to be handled is placed on 5mm thickness PP On plate, glass surrounding is touched with tape, ink surface need to be printed when preventing frosting from handling and is etched to.
Further, in the S2, sulfuric acid is the technical grade sulfuric acid of concentration 98%, and hydrofluoric acid is the industry of concentration 55% Stage hydrofluoric acid.
Further, in the S3, standing time is 2 minutes.
Further, in S5, removal sealing means are to tear edge sealing adhesive band, are then placed in the cleaning of plate cleaning machine.
Further, in the S6, silk-screen ink print steps are divided into four printings.
The first printing are as follows: get upper right side keypad mark silk-screen screen frame and be located on printing machine platform, by printing apparatus Positioning is placed on board and fixes, and clear glass is face-up, is put into jig, carries out the first printing with the first ink.
The second printing are as follows: get full version silk-screen screen frame and be located on printing machine platform, printing apparatus positioning is placed in machine It is on platform and fixed, clear glass is face-up, it is put into jig, carries out the second printing with the second ink.
The third printing are as follows: get the halftone with character and be erected on printing machine platform, printing apparatus positioning is placed in It is on board and fixed, clear glass is face-up, it is put into jig, carries out the third printing with third ink.
4th printing are as follows: get the reinforcement halftone that character extends out and be erected on printing machine platform, printing apparatus is positioned and is put It is put on board and fixed, clear glass is face-up, it is put into jig, carries out the 4th printing with the 4th ink.
The beneficial effects of the present invention are: the present invention solves asking for the slide-mouse semi-transparent place's color color difference of glass traditional handicraft Topic, switch between the numeric keypad when full page color made and lighting more naturally, visual effect greatly promotes.
Specific embodiment
The present invention is further explained in the light of specific embodiments, so that those skilled in the art can be better Understand the present invention and can be practiced, but illustrated embodiment is not as a limitation of the invention.
The present invention a kind of electric slide-mouse glass-making processes, comprising the following steps: S1. does a surface of original sheet glass close Envelope processing, original sheet glass it is another surface exposed.
S2. the surface exposed using pretreatment fluid cleaning original sheet glass, pretreatment fluid includes with weight institute at assignment system The hydrofluoric acid of the sulfuric acid of 10%-15%, 5%-10% that accounting example calculates, remaining be water.For example, in pretreatment fluid, sulfuric acid Weight accounts for the 12% of overall weight, and the 8% of hydrofluoric acid weight overall weight, the weight of water accounts for the 80% of overall weight.
S3. by the original sheet glass handled be put into frosting chemical pond carry out frosting etching process, standing time be 1 minute extremely 3 minutes, the ingredient configuration of frosting liquor included 40% hydrogen fluoride ammonia, 10% barium sulfate calculated with weight proportion, 20% sulfuric acid, remaining is water.
S4. the original sheet glass after frosting is rinsed with water completely, is put into chemical polishing solution and carries out attenuated polishing, when placement Between be 1 minute to 5 minutes, the configuration of the ingredient of chemical polishing solution includes the hydrogen fluorine of the 60%-70% calculated with weight proportion Acid, remaining is water.For example, standing time can be 2 minutes or 3.5 minutes, in chemical polishing solution, hydrogen fluorine in aforementioned S4 Sour weight accounts for the 65% of overall weight, and water weight accounts for the 35% of overall weight.
Since glass single-sided is in frosted finish effect after frosting, the transmitance of glass itself is weakened it is more, carry on the back after printing ink from The bright-coloured degree and brightness that the observation of frosting face is showed have larger impact.By after above-mentioned polishing process for glass Transmitance promoted, conducive to the presentation of back up ink colors, transmitance reduces bring shadow after effective solution frosting It rings, makes product more diversification in the adjustment of sense of touch and color.
S5. the original sheet glass after polishing is removed into sealing, rinsed well.
The sharp processing of rear workshop section is done according to the size and color of actual requirement by the above-mentioned glass processed, such as Chemical tempering, the processing such as silk-screen printing.Silk-screen printing is the important step of mobile phone and pen electricity display screen outline border, is a kind of will have one The ink for determining color, by printing pattern, words transfer printing on the substrate.Ink mainly by pigment, binder, filler material and The uniform mixture of the material compositions such as auxiliary material.
S6. silk-screen ink prints: silk-screen screen frame being located on printing machine platform, printing apparatus positioning is placed on board And it is fixed, bright by original sheet glass is put into jig up, is repeatedly printed with ink;Done in S1 close in clear glass face Seal the one side of processing.
S7. the glass after the completion of silk-screen is put into oven and is toasted, baking temperature is 150 degrees Celsius, baking time 10- 15 minutes, for example can be 11 minutes, 12 minutes, 13 minutes, 14 minutes.
In the S1, the mode of encapsulation process are as follows: the original sheet glass that need to be handled is placed on 5mm thickness PP plate, it will Glass surrounding is touched with tape, and ink surface need to be printed when preventing frosting from handling and is etched to.
In the S2, sulfuric acid is the technical grade sulfuric acid of concentration 98%, and hydrofluoric acid is the industrial stage hydrofluoric acid of concentration 55%.
In the S3, standing time is 2 minutes.
In S5, removal sealing means are to tear edge sealing adhesive band, are then placed in the cleaning of plate cleaning machine.
In the S6, silk-screen ink print steps are divided into four printings.Specifically, the first printing are as follows: get upper right Square keypad mark silk-screen screen frame is located on printing machine platform, and printing apparatus positioning is placed on board and is fixed, by glass It is bright face-up, it is put into jig, carries out the first printing with the first ink.First ink is blue ink, specially SNX- GLS-100031 (imperial family is blue)-PT1 (upper right corner keypad) ink.
The second printing are as follows: get full version silk-screen screen frame and be located on printing machine platform, printing apparatus positioning is placed in machine It is on platform and fixed, clear glass is face-up, it is put into jig, carries out the second printing with the second ink.Second ink is blue Ink, specially SNX-GLS-100031-PT2 (body color/imperial family is blue) ink.
The third printing are as follows: get the halftone with character and be erected on printing machine platform, printing apparatus positioning is placed in It is on board and fixed, clear glass is face-up, it is put into jig, carries out the third printing with third ink.Third ink is ash Color ink, specially SNX-GLS-100031-PT3 (keyboard grey) ink.
4th printing are as follows: get the reinforcement halftone that character extends out and be erected on printing machine platform, printing apparatus is positioned and is put It is put on board and fixed, clear glass is face-up, it is put into jig, carries out the 4th printing with the 4th ink.4th ink For black ink, specially SNX-GLS-100031-PT4 (base black) ink.
In other embodiments, according to product needs, silk-screen ink print steps can be divided into it is secondary, three times, five times, Six is inferior, and printing the ink colors used every time can also be replaced according to actual needs.
It can achieve by the control of above-mentioned glass silk screen printing technique ink and print order when not turning on light, ink, which has, to be hidden Effect.I.e. in actual use, when do not turn on be arranged on notebook for slide-mouse glass provide lighting effects lamp when, meat Eye is not observe the symbols such as number on numeric keypad, realizes the concealment effect of numeric keypad, and uses traditional handicraft raw Numeric keypad on the slide-mouse glass of production is in non-polishing and high-visible.When lamp is opened, use is produced by the invention Product can be clearly seen that the symbol on slide-mouse glass on numeric keypad, and by above-mentioned chemical polishing later for glass Transmitance promoted, effectively solving transmitance after frosting for the presentation of back up ink colors reduces bring shadow It rings, makes product more diversification in the adjustment of sense of touch and color.
Compared with prior art, the present invention is adjusted by etching solution ingredient to glass surface treatment and formula first It is whole, to form different surfaces crystal form to control glass frosting surface roughness size after etching, by using strong acid chemical after etching Attenuated polishing controls the height of the transmitance of product, and the surface crystal form after making frosting is rendered as rule by irregular polygon Ball-type, reduce the refraction of light to increase the permeability of glass.
Secondly, modulating body color in glass cross printing process with the semi-transparent ink of whole face IR, cooperating keyboard ink lid Bottom makes product show the whole face colors of needs.
Traditional handicraft prints IR half by the way of hollowed printing at the numeric keypad for needing to present semi-transparent lighting effects Saturating ink, and manufacture craft of the invention solves the problems, such as the semi-transparent place's color color difference of traditional handicraft, the full page color and point made Switch between numeric keypad when lamp more naturally, visual effect greatly promotes.
Embodiment described above is only to absolutely prove preferred embodiment that is of the invention and being lifted, protection model of the invention It encloses without being limited thereto.Those skilled in the art's made equivalent substitute or transformation on the basis of the present invention, in the present invention Protection scope within.Protection scope of the present invention is subject to claims.

Claims (6)

1. a kind of electric slide-mouse glass-making processes, which comprises the following steps:
S1. encapsulation process is done on a surface of original sheet glass, original sheet glass it is another surface exposed;
S2. the surface exposed using pretreatment fluid cleaning original sheet glass, pretreatment fluid includes with weight institute accounting at assignment system The hydrofluoric acid of the sulfuric acid of 10%-15%, 5%-10% that example calculates, remaining be water;
S3. the original sheet glass handled is put into frosting chemical pond and carries out frosting etching process, standing time is 1-3 minutes, is covered Sand liquid ingredient configuration include with weight proportion calculate 40% hydrogen fluoride ammonia, 10% barium sulfate, 20% sulfuric acid, Remaining is water;
S4. the original sheet glass after frosting is rinsed with water completely, is put into chemical polishing solution and carries out attenuated polishing,
Standing time is -5 minutes 1 minute, and the ingredient configuration of chemical polishing solution includes the 60%- calculated with weight proportion 70% hydrofluoric acid, remaining is water;
S5. the original sheet glass after polishing is removed into sealing, rinsed well;
S6. silk-screen ink prints: silk-screen screen frame being located on printing machine platform, printing apparatus positioning is placed on board and is consolidated Fixed, bright by original sheet glass is put into jig up, is printed with ink;
S7. the glass after the completion of silk-screen is put into oven and is toasted, baking temperature is 150 degrees Celsius, and baking time is 10-15 points Clock.
2. pen electricity slide-mouse glass-making processes according to claim 1, which is characterized in that in the S1, encapsulation process Mode are as follows: the original sheet glass that need to be handled is placed on 5mm thickness PP plate, glass surrounding is touched with tape, is prevented Ink surface need to be printed when frosting processing to be etched to.
3. pen electricity slide-mouse glass-making processes according to claim 2, which is characterized in that in the S2, sulfuric acid is dense The technical grade sulfuric acid of degree 98%, hydrofluoric acid are the industrial stage hydrofluoric acid of concentration 55%.
4. pen electricity slide-mouse glass-making processes according to claim 3, which is characterized in that in the S3, standing time It is 2 minutes.
5. pen electricity slide-mouse glass-making processes according to claim 4, which is characterized in that in S5, remove sealing means To tear edge sealing adhesive band, it is then placed in the cleaning of plate cleaning machine.
6. pen electricity slide-mouse glass-making processes according to claim 5, which is characterized in that in the S6, silk-screen ink Print steps are divided into four printings;
The first printing are as follows: get upper right side keypad mark silk-screen screen frame and be located on printing machine platform, printing apparatus is positioned It is placed on board and fixed, clear glass is face-up, it is put into jig, carries out the first printing with the first ink;
The second printing are as follows: get full version silk-screen screen frame and be located on printing machine platform, printing apparatus positioning is placed on board And it is fixed, clear glass is face-up, it is put into jig, carries out the second printing with the second ink;
The third printing are as follows: get the halftone with character and be erected on printing machine platform, printing apparatus positioning is placed in board It goes up and fixes, clear glass is face-up, it is put into jig, carries out the third printing with third ink;
4th printing are as follows: get the reinforcement halftone that character extends out and be erected on printing machine platform, printing apparatus positioning is placed in It is on board and fixed, clear glass is face-up, it is put into jig, carries out the 4th printing with the 4th ink.
CN201811384789.XA 2018-11-20 2018-11-20 Method for manufacturing pen-power mouse glass Active CN109399948B (en)