CN109202223A - A kind of method of multi-layer sintering net Gas Tungsten Arc Welding - Google Patents
A kind of method of multi-layer sintering net Gas Tungsten Arc Welding Download PDFInfo
- Publication number
- CN109202223A CN109202223A CN201811084372.1A CN201811084372A CN109202223A CN 109202223 A CN109202223 A CN 109202223A CN 201811084372 A CN201811084372 A CN 201811084372A CN 109202223 A CN109202223 A CN 109202223A
- Authority
- CN
- China
- Prior art keywords
- welding
- sintered meshwork
- edge
- welding rod
- rod
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Pending
Abstract
The present invention relates to a kind of methods of multi-layer sintering net Gas Tungsten Arc Welding, comprising: the first step processes the welding rod as packing material;Second step assembles welding rod in sintered meshwork edge fit to be welded;Third step carries out positioning welding using tungsten argon arc soldering method;4th step carries out tape edge to sintered meshwork welding edge using Tig Welding welding rod and the sintered meshwork of not filling silk;5th step will be assembled into docking form by the sintered meshwork of tape edge, and use argon tungsten-arc welding positioning welding;6th step, Tig Welding pass through the sintered meshwork of tape edge processing, sintered meshwork are welded into the shape of needs.Tape edge is carried out in advance to sintered meshwork welding edge by the method for preset welding rod, efficiently solve sintered meshwork in direct butt welding be easy burn scrap, the problem that welding efficiency is low, it is easy to operate, it is adaptable.
Description
Technical field
The present invention relates to welding field, the method for specifically a kind of multi-layer sintering net Gas Tungsten Arc Welding.
Background technique
Multi-layer sintering net is formed by composite steel silk screen sintering, main filtration, for the filter screen of filter, due to
Phenomena such as filter has shape need to sintered meshwork, and while being sintered net forming is easy to happen fracture of wire, delamination, limits sintered meshwork
Shape needs to realize the molding of sintered meshwork by welding.
Since sintered meshwork is layer structure, every layer of steel wire diameter is also different, is easy to burn when directly being welded, make
Fracture of wire into the net, and welding process is high to the skill requirement of welder, welding efficiency is low, and qualification rate is low, weldquality stability
Difference needs to improve welding technique.
Summary of the invention
The present invention aiming at the above shortcomings existing in the prior art, provides a kind of multi-layer sintering net Gas Tungsten Arc Welding
Method carries out tape edge to sintered meshwork welding edge by the method for preset welding rod in advance.
The present invention is achieved by the following technical solutions, a kind of method of multi-layer sintering net Gas Tungsten Arc Welding, including
Following steps:
The first step processes the preset welding rod as packing material;
Second step assembles welding rod in sintered meshwork edge fit to be welded;
Third step carries out positioning welding using tungsten argon arc soldering method;
4th step carries out tape edge to sintered meshwork welding edge using Tig Welding welding rod and the sintered meshwork of not filling silk;
5th step will be assembled into docking form by the sintered meshwork of tape edge, and use argon tungsten-arc welding positioning welding;
6th step, Tig Welding pass through the sintered meshwork of tape edge processing, sintered meshwork are welded into certain shape.
Further, preset welding rod of the processing as packing material in the first step, it is desirable that material and sintering net materials one
It causes, for welding rod with a thickness of 1.5mm, welding rod length is consistent with sintered meshwork welding edge lengths, and welding rod width is 3mm;
Further, welding rod is compressed using tooling in the second step, welding rod end face need to be aligned with sintered meshwork welding edge, weldering
Item need to expose 1.5~2mm;
The method of multi-layer sintering net Gas Tungsten Arc Welding of the invention, compared with prior art, the advantage is that:
One, sintered meshwork welding edge is carried out by tape edge by using preset welding wire, then realizes the welding of sintered meshwork, it can be effective
Solder yield is improved, sintered meshwork is improved and directly welds the problem of burning.
Two, the method for multi-layer sintering net Gas Tungsten Arc Welding proposed by the present invention, it is easy to operate, it is adaptable, it is high-efficient.
Detailed description of the invention
Fig. 1 is the schematic illustration of the multi-layer sintering net tungsten argon arc welding method of proposition of the invention;
Fig. 2 is the molding assembling schematic diagram of sintered meshwork of the embodiment of the present invention;
Fig. 3 is the flow chart of multi-layer sintering net tungsten argon arc welding method of the invention.
Specific embodiment
Elaborate below to the embodiment of the present invention: the present embodiment carries out under the premise of the technical scheme of the present invention
Implement, the detailed implementation method and specific operation process are given, but protection scope of the present invention is not limited to following implementation
Example.
As shown in Figure 1, multi-layer sintering net tungsten argon arc welding method provided in this embodiment, includes the following steps:
The first step processes the preset welding rod 2 as packing material;
Second step, by the assembly of welding rod 2 in the edge fit to be welded of sintered meshwork 1, and it is fixed using compression tooling 3;
Third step carries out positioning welding, the position of fixed welding rod 2 and 1 welding edge of sintered meshwork using tungsten argon arc soldering method;
4th step carries out tape edge to sintered meshwork welding edge using Tig Welding welding rod and the sintered meshwork of not filling silk;
5th step will be assembled into docking form by the sintered meshwork of tape edge, and use argon tungsten-arc welding positioning welding;
6th step, Tig Welding pass through the sintered meshwork of tape edge processing, form weld seam 4, sintered meshwork is welded into one
Fixed shape.
Specifically:
The first step processes preset welding rod as packing material, it is desirable that material is consistent with net materials are sintered, welding rod with a thickness of
1.5mm, welding rod length is consistent with sintered meshwork welding edge lengths, and welding rod width is 3mm;
Second step is compressed welding rod using tooling, and welding rod end face need to be aligned with sintered meshwork welding edge, and welding rod need to expose 1.5
~2mm, as shown in Figure 1;
Third step carries out positioning welding using tungsten argon arc soldering method, is welded using the fixed welding rod 2 of press strip 3 and sintered meshwork 1
The position on side, welding current 30A position spot diameter≤φ 4mm, height≤0.5mm, spacing 30mm~50mm;
4th step carries out tape edge, weldering to sintered meshwork welding edge using Tig Welding welding rod and the sintered meshwork of not filling silk
Afterwards as shown in Figure 1;
5th step will be assembled into docking form by the sintered meshwork of tape edge, and use argon tungsten-arc welding positioning welding, welding
Electric current 30A positions spot diameter≤φ 4mm, height≤0.5mm, spacing 30mm~50mm;
6th step, Tig Welding pass through the sintered meshwork of tape edge processing, form weld seam 4, sintered meshwork is welded into one
Fixed shape, as shown in Figure 2.
After the above method welds, the high-quality and high-efficiency welding of filter screen is realized.
Specific embodiments of the present invention are described above.It is to be appreciated that the invention is not limited to above-mentioned
Particular implementation, those skilled in the art can make various deformations or amendments within the scope of the claims, this not shadow
Ring substantive content of the invention.
Claims (5)
1. a kind of method of multi-layer sintering net Gas Tungsten Arc Welding, which comprises the steps of:
The first step processes the preset welding rod as packing material;
Second step assembles welding rod in sintered meshwork edge fit to be welded;
Third step carries out positioning welding using tungsten argon arc soldering method;
4th step carries out tape edge to sintered meshwork welding edge using Tig Welding welding rod and the sintered meshwork of not filling silk;
5th step will be assembled into docking form by the sintered meshwork of tape edge, and use argon tungsten-arc welding positioning welding;
6th step, Tig Welding pass through the sintered meshwork of tape edge processing, sintered meshwork are welded into certain shape.
2. a kind of method of multi-layer sintering net Gas Tungsten Arc Welding according to claim 1, it is characterised in that: described
The welding rod material processed in one step is consistent with sintering net materials, and welding rod welds side length with a thickness of 1.5mm, welding rod length and sintered meshwork
Degree is consistent, and welding rod width is 3mm.
3. a kind of method of multi-layer sintering net Gas Tungsten Arc Welding according to claim 1, it is characterised in that: described second
Welding rod is compressed using tooling in step, welding rod end face need to be aligned with sintered meshwork welding edge, and welding rod need to expose 1.5~2mm for welding
It connects.
4. a kind of method of multi-layer sintering net Gas Tungsten Arc Welding according to claim 1, it is characterised in that: the third
The position of press strip fixed welding rod and sintered meshwork welding edge, welding current 30A are used in step.
5. a kind of method of multi-layer sintering net Gas Tungsten Arc Welding according to claim 1, it is characterised in that: the described 4th
In step, using not welding with filler wire method, an anchor point is welded every 50~80mm.