CN109107771A - Combined capturing and collecting agent improves low-grade lead zinc-silver ore-dressing of polymetallic ore and refers to calibration method - Google Patents

Combined capturing and collecting agent improves low-grade lead zinc-silver ore-dressing of polymetallic ore and refers to calibration method Download PDF

Info

Publication number
CN109107771A
CN109107771A CN201810739820.0A CN201810739820A CN109107771A CN 109107771 A CN109107771 A CN 109107771A CN 201810739820 A CN201810739820 A CN 201810739820A CN 109107771 A CN109107771 A CN 109107771A
Authority
CN
China
Prior art keywords
zinc
lead
added
tailing
additional amount
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CN201810739820.0A
Other languages
Chinese (zh)
Inventor
高承康
袁龙潭
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Yunnan Gold Republic Resources Co Ltd
Original Assignee
Yunnan Gold Republic Resources Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Yunnan Gold Republic Resources Co Ltd filed Critical Yunnan Gold Republic Resources Co Ltd
Priority to CN201810739820.0A priority Critical patent/CN109107771A/en
Publication of CN109107771A publication Critical patent/CN109107771A/en
Pending legal-status Critical Current

Abstract

The invention belongs to technical field of beneficiation, and in particular to a kind of combined capturing and collecting agent improves low-grade lead zinc-silver ore-dressing of polymetallic ore and refers to calibration method.The present invention uses diethyldithiocarbamate for main collecting agent in lead process, butylamine black powder, 25# black powder be supplementary catching agent, zinc process ethyl xanthate and butyl xanthate according to the proportion of 1:1 as main collecting agent, butylamine black powder is as supplementary catching agent.By the use using combined capturing and collecting agent, in the case that concentrate grade is stablized or even improved by a small margin, the rate of recovery of three kinds of metals of lead zinc-silver is increased substantially, while improving content of the silver in lead concentrate, and economic benefit is obviously improved.

Description

Combined capturing and collecting agent improves low-grade lead zinc-silver ore-dressing of polymetallic ore and refers to calibration method
Technical field
The invention belongs to technical field of beneficiation, and in particular to a kind of combined capturing and collecting agent raising low-grade lead zinc-silver polymetallic ore The method of mineral processing index.
Background technique
The lead grade 0.6% or so of low-grade lead zinc-silver polymetallic ore, zinc grade 1.6% or so, silver-colored 70g/t or so are former Mine disseminated grain size is thinner, the sulfide minerals such as association pyrite, larger to mineral processing index interference.The prior art is sorting process In, using the single medicament such as xanthate or diethyldithiocarbamate as when collecting agent, using the single medicament such as xanthate or diethyldithiocarbamate as When collecting agent, although concentrate grade can achieve sale substantially and require: lead concentrate leaded 50% or so, zinc concentrate are left containing zinc 40% The right side, but xanthate have stronger subsequent collection performance but selectivity it is poor, diethyldithiocarbamate have stronger selectivity but subsequent collection performance compared with Xanthate is poor, and the rate of recovery of each metal is lower: the rate of recovery is lead zinc 80% to 85%, and total silver 75% to 80% is difficult to improve.
Summary of the invention
In view of the problems of the existing technology, the present invention provides a kind of combined capturing and collecting agent raising low-grade lead zinc silver polymetallic The method of mine mineral processing index, it is therefore an objective to by being applied in combination for two kinds of medicaments, in lead-zinc sulfide ore during sorting, sufficiently send out Respective advantage performance is waved, has certain selectivity while strengthening collecting, both ensure that the concentrate grade of lead zinc, simultaneously Greatly improve the rate of recovery.
Combined capturing and collecting agent of the invention improves low-grade lead zinc-silver ore-dressing of polymetallic ore and refers to calibration method, according to the following steps It carries out:
(1) low-grade lead zinc-silver polymetallic ore raw ore is milled to -200 mesh and accounts for 68% or more, be added lime adjust pH to 9.5, zinc sulfate and sodium sulfite stirring is added, zinc sulfate additional amount is 500g/t raw ore, and sodium sulfite additional amount is 500g/t, Then 25# black powder and butylamine stirring is added, 25# xanthate additional amount is 10g/t raw ore, is eventually adding diethyldithiocarbamate stirring, diethyldithiocarbamate Additional amount is 60g/t raw ore, obtains lead roughing mine and carries out lead roughing flotation, obtains lead rougher concentration and lead rougher tailings;
(2) lime is added into the lead rougher concentration and adjusts pH to 9.5, zinc sulfate and sodium sulfite is then added, The additional amount of zinc sulfate is 200g/t lead rougher concentration, and the additional amount of sodium sulfite is 200g/t lead rougher concentration, obtains lead essence Mine and lead tailing;30g/t diethyldithiocarbamate is added into lead rougher tailings, obtains lead and scans mine, lead, which is scanned, to be obtained lead after mine is scanned and sweep Concentrate selection and lead scan tailing;The lead tailing and lead scavenger concentrate return to lead roughing flotation;
(3) it is scanned to lead and lime adjusting pH to 10.5 is added in tailing, copper sulphate stirring is added, copper sulphate additional amount is 250g/t lead scans tailing, and butyl xanthate and ethyl xanthogenate is then added, and the additional amount of butyl xanthate is that 40g/t lead scans tailing, lead ethyl xanthate The additional amount of medicine is that 40g/t lead scans tailing, obtains zinc roughing mine and carries out zinc roughing flotation, obtains zinc rougher concentration and zinc roughing Tailing;
(4) it is added lime into zinc rougher concentration, adjusts pH to 11.5, obtain that zinc is selected rough, and zinc is selected rough through floating Choosing obtains zinc concentrate and zinc cleaner tailing;Copper sulphate stirring is added into zinc rougher tailings, copper sulphate additional amount is 100g/t zinc Butyl xanthate and ethyl xanthogenate stirring is added in rougher tailings, and butyl xanthate additional amount is 20g/t zinc rougher tailings, and ethyl xanthogenate additional amount is 20g/t zinc rougher tailings is eventually adding butylamine, and butylamine additional amount is 20g/t zinc rougher tailings, obtains zinc and scans mine, zinc is scanned Mine obtains zinc scavenger concentrate and tailing after scanning, wherein zinc scavenger concentrate and zinc cleaner tailing return to zinc roughing flotation stream jointly Journey;
(5) silver is recycled from lead concentrate and zinc concentrate.
Silver is association in lead zinc and other sulphide ores, can only be by the recycling to sulphide ores such as lead zinc to realization pair The recycling of silver to being separately separated for silver is realized in smelting link.But metal values of the silver in different minerals are widely different, The rate of recovery silver-colored in lead concentrate should be improved as far as possible.
Compared with prior art, the features of the present invention and beneficial effect are:
The present invention passes through being applied in combination for two kinds of medicaments, and in lead-zinc sulfide ore during sorting, two kinds of medicaments are sufficiently sent out Respective advantage performance is waved, has certain selectivity while strengthening collecting, both ensure that the concentrate grade of lead zinc, is recycled Rate has also obtained certain amplitude raising.
The present invention uses diethyldithiocarbamate for main collecting agent in lead process, and butylamine black powder, 25# black powder are supplementary catching agent, zinc Process ethyl xanthate and butyl xanthate are according to the proportion of 1:1 as main collecting agent, and butylamine black powder is as supplementary catching agent.Pass through Using the use of combined capturing and collecting agent, in the case that concentrate grade is stablized or even is improved by a small margin, the recycling of three kinds of metals of lead zinc-silver Rate increases substantially, while improving content of the silver in lead concentrate, and economic benefit is obviously improved.
For the present invention in the case where reagent cost is basically unchanged, mineral processing index has raising by a relatively large margin, lead concentrate product Position 50% or so, the rate of recovery of lead are improved from 86% to 91%, and the silver-colored rate of recovery is improved from 45% to 52% in lead concentrate;Zinc essence Mine grade 40% or so, the rate of recovery of zinc are improved from 87% to 90%, and the silver-colored rate of recovery is improved from 35% to 37% in zinc concentrate.
Various medicaments are applied in combination, and corresponding beneficiation reagent cost is basically unchanged, or even reduce about 0.5 yuan/ton, ore dressing After the rate of recovery improves, the output value monthly increases 400,000 yuan.
Detailed description of the invention
Fig. 1 is the method and process process that combined capturing and collecting agent of the present invention improves low-grade lead zinc-silver ore-dressing of polymetallic ore index Figure.
Specific embodiment
The technical solution of the application is described further combined with specific embodiments below.
Embodiment 1
Combined capturing and collecting agent in the present embodiment improves low-grade lead zinc-silver ore-dressing of polymetallic ore and refers to calibration method, according to following Step carries out:
(1) low-grade lead zinc-silver polymetallic ore raw ore is milled to -200 mesh and accounts for 68% or more, be added lime adjust pH to 9.5, zinc sulfate and sodium sulfite stirring is added, zinc sulfate additional amount is 500g/t raw ore, and sodium sulfite additional amount is 500g/t, Then 25# black powder and butylamine stirring is added, 25# xanthate additional amount is 10g/t raw ore, is eventually adding diethyldithiocarbamate stirring, diethyldithiocarbamate Additional amount is 60g/t raw ore, obtains lead roughing mine and carries out lead roughing flotation, obtains lead rougher concentration and lead rougher tailings;
(2) lime is added into the lead rougher concentration and adjusts pH to 9.5, zinc sulfate and sodium sulfite is then added, The additional amount of zinc sulfate is 200g/t lead rougher concentration, and the additional amount of sodium sulfite is 200g/t lead rougher concentration, obtains lead essence Mine and lead tailing;30g/t diethyldithiocarbamate is added into lead rougher tailings, obtains lead and scans mine, lead, which is scanned, to be obtained lead after mine is scanned and sweep Concentrate selection and lead scan tailing;The lead tailing and lead scavenger concentrate return to lead roughing flotation;
(3) it is scanned to lead and lime adjusting pH to 10.5 is added in tailing, copper sulphate stirring is added, copper sulphate additional amount is 250g/t lead scans tailing, and butyl xanthate and ethyl xanthogenate is then added, and the additional amount of butyl xanthate is that 40g/t lead scans tailing, lead ethyl xanthate The additional amount of medicine is that 40g/t lead scans tailing, obtains zinc roughing mine and carries out zinc roughing flotation, obtains zinc rougher concentration and zinc roughing Tailing;
(4) it is added lime into zinc rougher concentration, adjusts pH to 11.5, obtain that zinc is selected rough, and zinc is selected rough through floating Choosing obtains zinc concentrate and zinc cleaner tailing;Copper sulphate stirring is added into zinc rougher tailings, copper sulphate additional amount is 100g/t zinc Butyl xanthate and ethyl xanthogenate stirring is added in rougher tailings, and butyl xanthate additional amount is 20g/t zinc rougher tailings, and ethyl xanthogenate additional amount is 20g/t zinc rougher tailings is eventually adding butylamine, and butylamine additional amount is 20g/t zinc rougher tailings, obtains zinc and scans mine, zinc is scanned Mine obtains zinc scavenger concentrate and tailing after scanning, wherein zinc scavenger concentrate and zinc cleaner tailing return to zinc roughing flotation stream jointly Journey;
Wherein the low-grade lead zinc-silver polymetallic ore raw ore is five Kou Dongxuan factory raw ores, and grade is lower, and lead is 0.6% or so, zinc is 1.5% or so, and silver is 90g/t or so.
For lead concentrate grade obtained by final up to 50%, the rate of recovery of lead is 91%, in lead concentrate the silver-colored rate of recovery improve to 52%;Zinc concentrate grade is up to 40%, and the rate of recovery of zinc is to 90%, and the silver-colored rate of recovery is improved to 37% in zinc concentrate.
Above specific embodiment is only the preferred embodiment of this creation, all in this wound not to limit this creation Any modification, equivalent substitution, improvement and etc. done within the spirit and principle of work, should be included in this creation protection scope it It is interior.

Claims (1)

1. a kind of combined capturing and collecting agent, which improves low-grade lead zinc-silver ore-dressing of polymetallic ore, refers to calibration method, it is characterised in that according to following Step carries out:
(1) low-grade lead zinc-silver polymetallic ore raw ore is milled to -200 mesh and accounts for 68% or more, lime is added and adjusts pH to 9.5, Zinc sulfate and sodium sulfite stirring is added, zinc sulfate additional amount is 500g/t raw ore, and sodium sulfite additional amount is 500g/t, then 25# black powder and butylamine stirring is added, 25# xanthate additional amount is 10g/t raw ore, is eventually adding diethyldithiocarbamate stirring, and diethyldithiocarbamate is added Amount is 60g/t raw ore, obtains lead roughing mine and carries out lead roughing flotation, obtains lead rougher concentration and lead rougher tailings;
(2) lime is added into the lead rougher concentration and adjusts pH to 9.5, zinc sulfate and sodium sulfite, sulfuric acid is then added The additional amount of zinc is 200g/t lead rougher concentration, and the additional amount of sodium sulfite is 200g/t lead rougher concentration, obtain lead concentrate and Lead tailing;30g/t diethyldithiocarbamate is added into lead rougher tailings, obtains lead and scans mine, lead, which is scanned, to be obtained lead after mine is scanned and scan essence Mine and lead scan tailing;The lead tailing and lead scavenger concentrate return to lead roughing flotation;
(3) it is scanned to lead and lime adjusting pH to 10.5 is added in tailing, copper sulphate stirring is added, copper sulphate additional amount is 250g/t Lead scans tailing, and butyl xanthate and ethyl xanthogenate is then added, and the additional amount of butyl xanthate is that 40g/t lead scans tailing, and ethyl xanthogenate adds Entering amount is that 40g/t lead scans tailing, obtains zinc roughing mine and carries out zinc roughing flotation, obtains zinc rougher concentration and zinc rougher tailings;
(4) it is added lime into zinc rougher concentration, adjusts pH to 11.5, it is selected rough to obtain zinc, and zinc is selected rough to be obtained through flotation To zinc concentrate and zinc cleaner tailing;Copper sulphate stirring is added into zinc rougher tailings, copper sulphate additional amount is the roughing of 100g/t zinc Butyl xanthate and ethyl xanthogenate stirring is added in tailing, and butyl xanthate additional amount is 20g/t zinc rougher tailings, and ethyl xanthogenate additional amount is 20g/t Zinc rougher tailings is eventually adding butylamine, and butylamine additional amount is 20g/t zinc rougher tailings, obtains zinc and scans mine, zinc is scanned mine and scanned After obtain zinc scavenger concentrate and tailing, wherein zinc scavenger concentrate and zinc cleaner tailing return to zinc roughing flotation flowsheet jointly;
(5) silver is recycled from lead concentrate and zinc concentrate.
CN201810739820.0A 2018-07-06 2018-07-06 Combined capturing and collecting agent improves low-grade lead zinc-silver ore-dressing of polymetallic ore and refers to calibration method Pending CN109107771A (en)