CN109099260A - A kind of steel modeling slip casting multiple tube for fluid heating snow melt - Google Patents
A kind of steel modeling slip casting multiple tube for fluid heating snow melt Download PDFInfo
- Publication number
- CN109099260A CN109099260A CN201810938796.3A CN201810938796A CN109099260A CN 109099260 A CN109099260 A CN 109099260A CN 201810938796 A CN201810938796 A CN 201810938796A CN 109099260 A CN109099260 A CN 109099260A
- Authority
- CN
- China
- Prior art keywords
- pipe
- slip casting
- multiple tube
- plastic inner
- snow melt
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Granted
Abstract
The invention discloses a kind of preparation methods of steel modeling slip casting multiple tube for fluid heating snow melt, steel modeling slip casting multiple tube is by plastic inner pipe, metal outer pipe and is formed between plastic inner pipe and metal outer pipe by slip casting and fills up the concrete layer in space between the two and is constituted, which comprises provides the metal outer pipe;The plastic inner pipe is provided, and plastic inner pipe is placed among metal outer pipe;With press mortar or grouting material be provided, and by its pressure injection between the plastic inner pipe and metal outer pipe in space, to form the concrete layer.
Description
Technical field
The present invention relates to pavement snow melting technical fields, multiple more particularly to a kind of steel modeling slip casting for fluid heating snow melt
Close pipe.
Background technique
It is using dynamical system that the energy of external heat source is flexibly defeated as carrier progress using hot fluid that fluid heats snow-melting system
It is equipped with realization snow melt, compared with dispensing the passive snow melt mode such as Chemical deicers, mechanical deicing's snow method, fluid heats snow melt system
System can carry out preventative active according to snowfall and weather condition and remove the snow, and system controllability and measurability is strong, energy utilization rate is high, heat source is wide
General (can be conventional heat sources or renewable heat source), simple installation.
It is to recycle hot fluid in the pipeline being embedded in inside face that fluid, which heats snow-melting system, is passed through
Heat convection heat exchange method at tube wall makes the heat transfer of fluid give road face structure, will by the heat transfer inside structure sheaf
Heat transfer is to road body surface face, and then logical heat transfer and ice and snow carry out heat exchange, to achieve the purpose that deicing or snow melting.Herein
In system, the low-freezings solution such as aqueous solution of propylene glycol, glycol water can be used as circulatory mediator;And it is embedded in face and works as
In tubing, good heatproof, corrosion resistance and good intensity and flexibility are needed, so as in construction and installation
Cheng Dangzhong and using working stage there is good resistances tube fluid to corrode and resist pavement loading such as automobile, winged
The ability of machine load action.
Currently, fluid heating pipeline tubing generally has metal tube such as steel pipe, PSP steel-plastics composite pipe and plastic tube etc..
Steel pipe has intensity height, and linear expansion coefficient and concrete are close, is mainly used for heat donor fluid conveying and uses, thermal conductivity
It can be strong.But since fluid generally adds anti-icing fluid, there is microcorrosion, therefore steel pipe is not suitable for making directly as heating tube
With.
It is raw material that plastic tube, which is usually with synthetic resin, that is, polyester, stabilizer, lubricant, plasticizer is added etc., with
The method of " modeling " forms in tuber through extrusion process, be mainly used as building construction tap water supply system piping, draining,
Exhaust and blowdown sanitary pipe, subsoil drain system, rain pipe and electric wire install matched penetration pipe etc..Plastic tube, point
For thermoplastic pipes and thermosetting plastics pipe two major classes.Belonging to thermoplastic has polyvinyl chloride pipe, polyethylene pipe, polypropylene
Pipe, polyformaldehyde pipe etc.;Belonging to heat cured has phenola plastics pipe etc..The major advantage of plastic tube be good corrosion resisting property, light weight, at
Type convenience, handling ease, the pipeline flexibility of thermoplastics type and ductility are relatively preferable;But the heating conduction of plastic tube and anti-folding
Compressive property is poor.The impact force of traffic loading is larger on blocking the way face or pavement slab between faulting of slab ends quiet shifting when, the resistance of plastic tube
Ability is weaker, there is the risk for being cut off and forming leakage.
PSP steel-plastic composite pressure pipe is novel metal and the compound tubing of plastics, interior generally using welded still pipe as middle layer
Outer layer is vinyon, using hot melt adhesive special, the tubing being combined into one by extruding forming method.The tubing overcomes
Easy-to-rust existing for steel pipe, have pollution, heaviness, service life it is short it is low with intensity existing for plastic tube, swell increment is big, easily-deformable
Defect, and the Common advantages with steel pipe and plastic tube, if oxygen barrier is good, has higher rigidity, underground pipe is easy detection etc..
But PSP steel-plastics composite pipe there are integral strengths smaller, the poor disadvantage of heating conduction.In addition when using PSP steel-plastics composite pipe
When, to long-distance transmission pipeline, longest 12m need to have hot melt or electric fusion joint at one, by taking F class runway designs width 60m as an example,
Need connector at least 4.If needing connector at one at 5m in conjunction with runway working procedure, 60m is needed at least 11
Connector.More connector will cause fluid leakage risk.
Therefore, it is necessary to novel pipelines, and to solve, above-mentioned there are technical problems.
Summary of the invention
In order to overcome disadvantage mentioned above, it is an object of that present invention to provide a kind of steel modeling slip casting for fluid heating snow melt is compound
Pipe and preparation method, the multiple tube long service life, corrosion resistance is strong, small on the influence of the fracture resistance of concrete road surface,
Heating conduction is strong.
According to an aspect of the present invention, a kind of preparation side of steel modeling slip casting multiple tube for fluid heating snow melt is provided
Method, the steel modeling slip casting multiple tube are formed in plastic inner pipe and metal outer pipe by plastic inner pipe, metal outer pipe and by slip casting
Between and fill up the concrete layer in space between the two and constituted, which comprises
The metal outer pipe is provided;
The plastic inner pipe is provided, and plastic inner pipe is placed among metal outer pipe;With
There is provided press mortar or grouting material, and by its pressure injection between the plastic inner pipe and metal outer pipe in space,
To form the concrete layer.
An embodiment according to the present invention, wherein the press mortar or grouting material comply with standard TB/T3192-
2008 or JTG/TF502011.
An embodiment according to the present invention, wherein the press mortar or grouting material include H-60 grouting agent.
An embodiment according to the present invention, wherein the pressure when pressure injection is about 1.0~1.4MPa, preferably
1.1~1.3MPa, more preferably 1.2MPa.
An embodiment according to the present invention, wherein the injection speed when pressure injection is about 0.3-0.7m/s, preferably
For 0.5m/s.
An embodiment according to the present invention, wherein the system of the steel modeling slip casting multiple tube for fluid heating snow melt
Preparation Method further includes blocking the both ends of the plastic tube, and water is injected in it before the pressure injection.
An embodiment according to the present invention, wherein the pressure for injecting water in the plastic tube is no more than 0.4MPA.
An embodiment according to the present invention, wherein the system of the steel modeling slip casting multiple tube for fluid heating snow melt
Preparation Method also further includes adding solids in the plastic tube before closure, such as add thinner mass such as steel wire,
For adjusting the weight of plastic tube.
According to another aspect of the present invention, a kind of steel modeling slip casting multiple tube for fluid heating snow melt is provided, by plastics
It inner tube 30, metal outer pipe 10 and is formed between plastic inner pipe and metal outer pipe by slip casting and fills up space between the two
Concrete layer 20 is constituted.
An embodiment according to the present invention, wherein the plastic inner pipe 30 is polyethylene pipe.
An embodiment according to the present invention, wherein the polyethylene pipe is De25 plastic tube.
An embodiment according to the present invention, wherein the metal outer pipe is DN32 steel pipe.
An embodiment according to the present invention, wherein the length of steel modeling slip casting multiple tube is 1-60 meters.
An embodiment according to the present invention, wherein steel modeling slip casting multiple tube is eccentric pipe, the plastic inner pipe
Cross section geometric center be not overlapped with the cross section geometric center of the metal outer pipe.
An embodiment according to the present invention, wherein the plastic inner pipe locally reclines with the metal outer pipe.
An embodiment according to the present invention, wherein press mortar used in slip casting or grouting material meet mark
Quasi- TB/T3192-2008 or JTG/TF502011.
An embodiment according to the present invention, wherein the press mortar or grouting material include H-60 grouting agent.
An embodiment according to the present invention, wherein the thermal coefficient of steel modeling slip casting multiple tube is greater than 1.0W/
Such as 2.0,3.0,4.0,5.0W/ (mK) etc. (mK),.
The invention solves many technical problems tubing that fluid heating snow-melting system was selected in the past present in, produces
Beneficial technical effect:
1) service life can be up to 50 years.The service life of plastic tube can be up to 50 years, therefore by the plastics of innermost layer
Pipe undertakes heating fluid conveying function, it can be achieved that the pipeline more than road face design period (generally 30 years) uses duration.
2) corrosion resistance is strong.Steel pipe corrosion resistance itself is weaker, is not suitable for conveying heating fluid, plastic tube corrosion resistant
Erosion ability is most strong, can be used for directly transporting fluid.Using steel pipe as the outer protective shell of plastic tube, mortar is filled between the two, it can
Further strengthen the intensity and resistance to corrosion of compound pipeline complex pipeline.
3) " steel moulds slip casting multiple tube " thermal coefficient of the invention is preferable, is much better than PSP pipe and plastic tube.It therefore can be real
Existing good heat transfer and snow melt effect.
Detailed description of the invention
Fig. 1 is the steel modeling slip casting composite pipe structure signal for fluid heating snow melt according to an embodiment of the invention
Figure.
Fig. 2 is the preparation side of the steel modeling slip casting multiple tube for fluid heating snow melt according to an embodiment of the invention
The flow diagram of method.
Fig. 3 is the structural representation that pipeline heating conduction is detected using sandbox model according to an embodiment of the invention
Figure.
Specific embodiment
Present invention is further described in detail in the following with reference to the drawings and specific embodiments, but not as to limit of the invention
It is fixed.
Fig. 1 is that the steel modeling slip casting composite pipe structure for fluid heating snow melt of an embodiment according to the present invention shows
It is intended to.As shown in Figure 1, steel modeling slip casting multiple tube includes three parts namely plastic inner pipe 30, metal outer pipe 10 and concrete
Layer 20, wherein the concrete layer 20 is formed between plastic inner pipe and metal outer pipe by slip casting and fills up sky between the two
Between, the high temperature fluid 40 for providing thermal energy is flowed in plastic inner pipe 30.
Metal outer pipe 10 for example can be steel pipe, such as DN32 steel pipe, specifically can according to need to select steel appropriate
Tubing type.The length of steel pipe and diameter etc. can select according to specific needs, such as when the longer length such as 60 of needs
More steel pipes can be carried out silk and connect or weld by meter Shi.Metal outer pipe 10 is used as outer layer pipe, can mould slip casting multiple tube for steel
Good intensity and protection are provided.
Plastic inner pipe 30 can be thermoplastic pipes and thermosetting plastics pipe, such as can be polyvinyl chloride pipe, poly- second
Alkene pipe, PA tube, polyformaldehyde pipe, phenola plastics pipe etc..The internal diameter and length of plastic tube, which can according to need, to be selected, example
If its internal diameter can be selected with the design discharge of snow melt fluid, but its outer diameter should be suitably less than above-mentioned metal outer pipe
Internal diameter.Such as difference between the two can be 5mm-20mm, such as 6mm, 7mm, 8mm, 10mm, 15mm etc..Art technology
Personnel can according to need to be readily selected diameter appropriate.The length of plastic inner pipe 30, which can according to need, comes appropriate section
It takes, such as 1m, 5m, 10m, 30m, 60m etc..
Such as 30 major advantage of plastic inner pipe is good corrosion resisting property, light weight, convenient formation, handling ease, thermoplastics type
Pipeline flexibility and ductility are relatively preferable.An embodiment according to the present invention, wherein the plastic inner pipe 30 is De25
Polyethylene pipe.
In order to ensure snow melt effect, enhancing is thermally conductive, and the present invention is between outer tube (steel pipe) and heating tube (plastic tube)
Void layer is filled closely knit.As shown in Figure 1, multiple tube of the invention further includes setting outside the plastic inner pipe 30 and metal
Concrete layer 20 between pipe 10.The concrete layer 20 can be formed between plastic inner pipe and metal outer pipe and be filled up by slip casting
Space between the two.Concrete layer 20 makes plastic inner pipe 30 fixed, also support is provided for metal outer pipe 10, so that multiple tube
It is firmer on the whole, realize the technologies effects such as resistance to compression shock resistance, corrosion-resistant strong, good heat conductivity and long service life
Fruit.
More specifically, concrete layer 20 of the invention utilizes press mortar or grouting material, through slip casting in plastics
It is formed between pipe 30 and metal outer pipe 10.Be perfused mud jacking after formed concrete layer 20 it is closely knit, without hollowing, bubble-free, and
Integrated piping is in close contact ungauged regions without deformation, the outer wall and injecting paste material of outer tube wall and inner tube.In addition, integrated piping is also
With good thermal conductivity, hence it is evident that managed better than plastic tube or PSP, such as the thermal coefficient that can have is greater than 1.0W/ (m
), such as 2.0W/ (mK), 3.0W/ (mK), 4.0W/ (mK), 5.0W/ (mK), 6.0W/ (mK) etc. K.
For this purpose, can for example preferably conform to those of standard TB/T3192-2008 or JTG/TF502011 press mortar or
Grouting material, more preferably those include the press mortar or grouting material of H-60 grouting agent.Based on the teachings of the present invention and combine
The prior art, those skilled in the art can be readily selected suitable press mortar or grouting material.
As shown in Figure 1, steel modeling slip casting multiple tube of the invention can be the section of eccentric pipe namely the plastic inner pipe 30
Geometric center is not overlapped with the cross section geometric center of the metal outer pipe 10.It means that concrete layer 20 is in plastic inner pipe 30
Thickness between metal outer pipe 10 is not uniform.Such as shown in figure, the thickness of concrete layer 20 from top to bottom gradually becomes
Small, upper thickness is less than the thickness of lower part.Further, the top section of plastic inner pipe 30 or even the metal outer pipe 10 that can recline
Inner wall.
When by such eccentric pipe according to embedment underground as shown in the figure, due to accommodating the plastic inner pipe 30 of high temperature fluid more
Add close to the metal outer pipe 10 that even reclines, therefore the heating conduction on the top of multiple tube is more preferable, is more easier thermal energy conduction extremely
Ground can be realized better snow melt effect.
The formation process of 2 the present invention is further explained multiple tubes with reference to the accompanying drawing.With reference to attached drawing 2, use of the invention
It may include steps of in the preparation method of the steel modeling slip casting multiple tube of fluid heating snow melt:
Firstly, providing metal outer pipe 10, can according to need to select metal pipe material appropriate such as DN32 steel pipe.Steel pipe
Length and diameter etc. can select according to specific needs, can will such as when needing longer such as 60 meters of length
More steel pipes are welded;
Plastic inner pipe 30 is provided, and plastic inner pipe is placed among metal outer pipe, such as De25 polyvinyl chloride can be provided
Whole plastic tube is carried out poling using the manually or mechanically modes such as traction by pipe.The diameter of plastic tube can be according to snow melt fluid
Design discharge selected, outer diameter is suitably less than the internal diameter of above-mentioned metal outer pipe.Such as difference between the two can be
5mm-30mm, such as 6mm, 7mm, 8mm, 10mm, 1mm, 20mm, 25mm etc..The length of plastic inner pipe 30 can be according to metal
The degree of outer tube intercepts, for example, can the length appropriate that metal outer pipe is slightly longer than, reserve plastic tube two sides end length, so as to
In subsequent operation;
There is provided press mortar or grouting material, and by its pressure injection between the plastic inner pipe and metal outer pipe in space,
To form the concrete layer 20 for being full of the space.Press mortar or grouting material can choose those and comply with standard TB/
The material of T3192-2008 or JTG/TF502011, preferably those include the press mortar or grouting material of H-60 grouting agent.It will
The press mortar or grouting material modulated is by grouting equipment indentation pipeline clearance layer (namely the plastic inner pipe and metal outer pipe
Between space).Can select grouting pressure appropriate as the case may be, for example, can for 1.0~1.4MPa, for example
1.1MPa,1.2MPa,1.3MPa.It can control injection speed, such as 0.3-0.7m/s, such as 0.5m/s appropriate or so, and
And with suitable control and slip casting time of every root canal can be selected, such as every root canal the slip casting time can at 1.5~3 minutes, 2~
2.5 minute.Grouting equipment is well known to those skilled in the art, and is not repeated herein.
Due to the comprehensive function of the gravity and buoyancy of fluid, plastic inner pipe 30 floats bias during slip casting, thus
Cause to be formed by steel modeling slip casting multiple tube to be outside the cross section geometric center and the metal of eccentric pipe namely the plastic inner pipe
The cross section geometric center of pipe is not overlapped or even the top of the plastic inner pipe and the inner wall of the metal outer pipe locally recline.When
When by such eccentric pipe according to embedment underground as shown in Figure 1, due to accommodating the plastic inner pipe 30 of high temperature fluid closer to very
To the metal outer pipe 10 that reclines, therefore the heating conduction on the top of multiple tube is more preferable, is more easier thermal energy conduction to ground, can
Realize better snow melt effect.
Preferably, further include according to the method for the present invention the both ends of the plastic inner pipe 30 are blocked before slip casting, and
Water is injected in it.The weight for injecting the adjustable plastic inner pipe of water, it is possible thereby to adjust bias of the plastic inner pipe in slip casting
Degree.Mass such as steel wire etc. can certainly be added in plastic inner pipe, to adjust the weight of plastic inner pipe, adjust inclined
Heart degree, thus it is even possible that multiple tube it is not eccentric.Meanwhile water filling additionally aids the inside pressure for keeping plastic inner pipe 30
Power prevents from flattening plastic inner pipe 30 during slip casting.,
Those skilled in the art should be readily appreciated that.It can choose water injection pressure appropriate, prevent water injection pressure excessively high and cause
Plastics tube swelling, such as the pressure of injection water can be no more than 0.4MPa.It, can be by the water in plastic tube after slurry condensation
Or other mass remove.
Below with reference to embodiment, the present invention is further explained.
Embodiment-preparation of steel modeling slip casting multiple tube and the detection of performance parameter
Material and parameter:
Metal outer pipe be DN32 welded still pipe, 24 meters of length, outer diameter 41.23mm, wall thickness 2.47mm;
Plastic inner pipe be De25 polyethylene pipe, 24 meters of length, outer diameter 24.57mm, wall thickness 3.1mm;
Injecting paste material: the weight ratio of 30:10:90 measures water, grouting agent (H-60), cement, reference standard TB/T3192-
2008;
Grouting pressure: about 1.2MPa, injection speed: about 0.5m/s or so;
Water is full of in plastic inner pipe, both ends block, overpressure about 0.4MPa;
Steel modeling slip casting multiple tube is prepared using method of the invention, multiple samples are averaged, finally obtained steel modeling note
The length for starching multiple tube is 2496mm, eccentricity 4mm;
In addition, comparing group using DN32 welded still pipe, De25 polyethylene pipe, De25PSP steel-plastics composite pipe.Each product
Performance parameter see the table below 1.
Table 1: different pipe performance contrast tables 1
Wherein, the detection of concrete flexural strength is according to GBT 50082-2009 " normal concrete long-term behaviour and durable
Method for testing performance standard " and GBT 50081-2002 " standard for test methods of mechanical properties of ordinary concrete " carry out, most
The present invention and the addition FC fiber of other control tubes are obtained eventually, add 28d concrete flexural strength after pipe: as shown above, this
The steel modeling slip casting multiple tube of invention shows preferable concrete flexural strength, higher than the requirement of design standard 5.0MPa, and
Performance is better than other most of control tubes.
The detection of heating conduction is as follows:
By test section (including steel of the present invention modeling slip casting multiple tube, DN32 welded still pipe, De25PSP steel-plastics composite pipe,
De25 polyethylene pipe) it is respectively embedded in the soil that thermal coefficient is 1.25W/m.K, pipeline center's wheelbase ground 1m utilizes perseverance
Tepidarium circulates 40 DEG C of temperature of hot water with the speed of 2.0m/s and 1.2m/s in the duct, in test section length side
Thermal resistance temperature sensor (tube wall temperature being measured, in Fig. 3 shown in bullet) and hot-fluid is respectively set in tube top, tube bottom to center
Sensor surveys piece;In soil right above away from tube top at 0.95m, 3 thermal resistance temperature sensing are arranged along pipeline section axial direction
Device (number 1,2,3 is spaced 0.3m, the soil moisture close to soil surface is measured, referring to attached drawing 3).
30 DEG C of environment temperature of test, by 3 hours stabilizations, temperature sensor numerical fluctuations were less than 0.5 DEG C.
Medium is flowed with the speed of 2m/s and 1.2m/s, the convection transfer rate flowed in computer tube.Heat exchange amount depends on
The temperature difference of tube wall and medium, in stage on-test, since tube wall and the medium temperature difference are larger, exchange heat it is more violent, developmental tube into
The medium temperature drop of outlet is obvious, and tube wall temperature is relatively stable after 3 hours, and with medium temperature temperature difference very little, heat transfer effect
It is suppressed.But heat exchange is still main means, relatively thin in view of structure, and heat transfer is not still principal element, and examination is covered in sandbox
The soil mass volumetric heat capacity tested around pipe is tabled look-up as 2J/g.cm3, sandbox peripheral air thermal coefficient is 0.02W/ (mK),
Much smaller than soil thermal conductivity 1.25W/ (mK), environment temperature is higher, be equivalent to sandbox carry out isothermal holding, can approximation recognize
Be under adiabatic condition for sandbox, when test single developmental tube 3 hours time to soil transmitting heat to soil temperature rise not
Obviously.
Testing result shows: being λ 25 when the comprehensive thermal coefficient in eccentric structure top of the invention is at 25 DEG C of mean temperature
=5.09W/ (mK);It is λ 25=2.37W/ (m when the comprehensive thermal coefficient in this eccentric structure lower part is at 25 DEG C of mean temperature
K)。
That is, the heating conduction of steel modeling slip casting multiple tube of the invention be better than PSP steel-plastics composite pipe, polyethylene pipe, with
And concrete, it is only second to steel pipe, therefore heating conduction is very good, is conducive to conduct heat.And eccentric structure is also advantageous to fluid
Heat transfer snow melt upwards.
Previous fluid heating snow melt pipe material selection is single, and there are some problems.The present invention solves fluid heating and melts
Avenge pipeline some FAQs, such as burn into connector leakage, on pavement condition influence, plastic pipe itself it is anti-shearing difference ask
Topic.
In addition, the present invention is eccentric pipe.Plastic conduit is under the pressure head of slurry on built-in plastic tube nature in process
It is floating, close to steel duct upper wall is even close to, causes heating conduction superior, be advantageous to heat transfer.
Inventive pipeline by length limitation, can not flexibly construct according to the construction demand in municipal road face, changeable.
The above is only the preferable embodiment of the present invention, not does in any form to technical solution of the present invention
Limitation.Any simple modification, form variation and modification are made to above embodiments according to the technical essence of the invention, fallen
Enter protection scope of the present invention.
Claims (10)
1. a kind of preparation method of the steel modeling slip casting multiple tube for fluid heating snow melt, the steel modeling slip casting multiple tube is by plastics
Inner tube, metal outer pipe and the coagulation that space between the two is formed between plastic inner pipe and metal outer pipe and filled up by slip casting
Soil layer is constituted, which comprises
The metal outer pipe is provided;
The plastic inner pipe is provided, and plastic inner pipe is placed among metal outer pipe;With
Press mortar or grouting material are provided, and by its pressure injection between the plastic inner pipe and metal outer pipe in space, with shape
At the concrete layer.
2. the preparation method of the steel modeling slip casting multiple tube according to claim 1 for fluid heating snow melt, wherein described
Press mortar or grouting material comply with standard TB/T3192-2008 or JTG/TF502011.
3. the preparation method of the steel modeling slip casting multiple tube according to claim 1 for fluid heating snow melt, wherein described
Press mortar or grouting material include H-60 grouting agent.
4. the preparation method of the steel modeling slip casting multiple tube according to claim 1 for fluid heating snow melt, wherein described
Pressure when pressure injection is about 1.0~1.4MPa.
5. the preparation method of the steel modeling slip casting multiple tube according to claim 1 for fluid heating snow melt, wherein described
Injection speed when pressure injection is about 0.3-0.7m/s.
6. it is according to claim 1 for fluid heating snow melt steel modeling slip casting multiple tube preparation method, further include
Before the pressure injection, the both ends of the plastic inner pipe are blocked, and water is injected in it.
7. the preparation method of the steel modeling slip casting multiple tube according to claim 6 for fluid heating snow melt, wherein in institute
The pressure for stating injection water in plastic inner pipe is no more than 0.4MPA.
8. it is according to claim 6 for fluid heating snow melt steel modeling slip casting multiple tube preparation method, further include
Solids is added in the plastic inner pipe before closure.
9. the preparation method of the steel modeling slip casting multiple tube according to claim 1 for fluid heating snow melt, wherein described
It is eccentric pipe, the cross section geometric center of the plastic inner pipe and the cross section geometric center of the metal outer pipe that steel, which moulds slip casting multiple tube,
It is not overlapped.
10. the preparation method of the steel modeling slip casting multiple tube according to claim 9 for fluid heating snow melt, wherein described
Plastic inner pipe locally reclines with the metal outer pipe.