CN108568582A - A kind of welding method of corrugated conduit - Google Patents

A kind of welding method of corrugated conduit Download PDF

Info

Publication number
CN108568582A
CN108568582A CN201810370844.3A CN201810370844A CN108568582A CN 108568582 A CN108568582 A CN 108568582A CN 201810370844 A CN201810370844 A CN 201810370844A CN 108568582 A CN108568582 A CN 108568582A
Authority
CN
China
Prior art keywords
welding
groove
pipeline
bellows
welding rod
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CN201810370844.3A
Other languages
Chinese (zh)
Inventor
王勇
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Tianjin Jun Yong Li Prestressed Products Co Ltd
Original Assignee
Tianjin Jun Yong Li Prestressed Products Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Tianjin Jun Yong Li Prestressed Products Co Ltd filed Critical Tianjin Jun Yong Li Prestressed Products Co Ltd
Priority to CN201810370844.3A priority Critical patent/CN108568582A/en
Publication of CN108568582A publication Critical patent/CN108568582A/en
Pending legal-status Critical Current

Abstract

The invention belongs to bellows manufacturing technology field more particularly to a kind of welding method of corrugated conduit, the first step, the inspections of pipeline, check whether the surface of pipeline has the defects of crackle, shrinkage cavity, folding, pipe;Second step:Cleaning, cleans pipeline with pipeline cleaning;Third walks, preheating, and using electric preheating, the heating of uniform stabilization is carried out to bellows;4th step, groove processing carry out groove processing to bellows;5th step, polishing, polishes to groove using sander;6th step, welding, on groove face in striking to gap, welding rod is set to make slight lateral swing in two root faces, when root face fusing iron liquid connects together with welding rod molten drop, sent on welding rod, electrode tip all reaches groove bottom edge at this time, the 2/3 of entire electric arc will be in combustion inner pipe, and first molten hole is formed, when overhead welding is to oblique overhead position arc manipulation, it is necessary to assure partly punch state, to oblique vertical position welding and downhand position, top arc welding can be used.

Description

A kind of welding method of corrugated conduit
Technical field
The invention belongs to bellows manufacturing technology field more particularly to a kind of welding methods of corrugated conduit.
Background technology
Bellows refers to the tubular elastomeric sensing element connected into along folding retractable direction with foldable wrinkle piece.Bellows Be widely used in instrument and meter, be mainly used for the measuring cell as pressure measuring instruments, convert pressure into displacement or Power.Ripple tube wall is relatively thin, and sensitivity is higher, and measurement range is tens of pas to tens of megapascal.Its open end is fixed, sealed end Increase elasticity in free state, and using the helical spring of auxiliary or reed.Along pipe under the action of internal pressure when work Sub- elongated lengthwise makes movable end generate the displacement with pressure at certain relationship.Movable end drives pointer that can directly indicate The size of pressure.Bellows, which usually combines with displacement sensor, constitutes output as the pressure sensor of electricity, also uses sometimes Make isolation element.Since the stretching, extension of bellows requires larger volume to change, its response speed is less than Bourdon tube.
Bellows includes mainly metal bellows, expansion bellow, corrugated tube, diaphragm and diaphragm capsule and metal hose etc.. Metal bellows is mainly used in the effects that compensation pipes thermal deformation, damping, absorption line sedimentation and deformation, is widely used in stone The industries such as change, instrument, space flight, chemical industry, electric power, cement, metallurgy.The other materials such as plastics bellows is worn in medium conveying, electric power There is irreplaceable role in the fields such as line, lathe, household electrical appliances.
When bellows-welding, weld joint on inner side argon-filled protection is a cumbersome problem, and when caliber is larger, pipeline is longer When, such as argon filling directly into pipe, it will largely waste argon gas, increase engineering cost.
Invention content
The present invention provides a kind of welding method of corrugated conduit, with solve waste argon gas mentioned above in the background art, The problem of increasing cost.
Technical problem solved by the invention is realized using following technical scheme:
A kind of welding method of corrugated conduit, includes the following steps:
The first step, the inspection of pipeline check whether the surface of pipeline has the defects of crackle, shrinkage cavity, folding, pipe;
Second step:Cleaning, cleans pipeline with pipeline cleaning;
Third walks, preheating, and using electric preheating, the heating of uniform stabilization is carried out to bellows;
4th step, groove processing carry out groove processing to bellows;
5th step, polishing, polishes to groove using sander;
6th step, welding, on groove face in striking to gap, makes welding rod make slight lateral swing in two root faces, when root face is molten When changing iron liquid and welding rod molten drop and connecting together, sending on welding rod, electrode tip all reaches groove bottom edge at this time, and the 2/3 of entire electric arc Will be in combustion inner pipe, and first molten hole is formed, when overhead welding is to oblique overhead position arc manipulation, it is necessary to assure state is partly punched, until Oblique vertical position welding and downhand position can use top arc welding;
7th step, it is anti-oxidation, in pipe away from each 100mm in weld bond both sides at, a pair of rubber slab connected with iron wire of setting, plate thickness is 3-5mm is supported inside and outside plate with clamping plate, the metal hose of an a diameter of 3-5mm is filled on one piece of closure plate wherein, is welded Argon filling in Shi Xiangguan after being soldered, is pulled out rubber slab by metal hose;
8th step after the completion of oxidation, using material package weld seam and weld seam both sides are protected, makes weld seam Slow cooling;
9th step cleans groove, then polished smooth with sander after cooling.
The angle of the groove is 20 ° -30 °.
Beneficial effects of the present invention are:
The technical program is so that fusion when welding is preferably protected, and save argon gas with rubber closure plate argon-filled protection method Dosage can be used adhesive tape to seal one section of nozzle in advance, and the fusion length for only reserving the welding of welder's one-time continuous is torn after being soldered this section The adhesive tape of equal length is opened, then welding again, and so on, until welding is completed, whole implementation effect is ideal, and is conducive to It promotes the use of on a large scale.
Specific implementation mode
A kind of welding method of corrugated conduit, includes the following steps:
The first step, the inspection of pipeline check whether the surface of pipeline has the defects of crackle, shrinkage cavity, folding, pipe;
Second step:Cleaning, cleans pipeline with pipeline cleaning;
Third walks, preheating, and using electric preheating, the heating of uniform stabilization is carried out to bellows;
4th step, groove processing carry out groove processing to bellows;
5th step, polishing, polishes to groove using sander;
6th step, welding, on groove face in striking to gap, makes welding rod make slight lateral swing in two root faces, when root face is molten When changing iron liquid and welding rod molten drop and connecting together, sending on welding rod, electrode tip all reaches groove bottom edge at this time, and the 2/3 of entire electric arc Will be in combustion inner pipe, and first molten hole is formed, when overhead welding is to oblique overhead position arc manipulation, it is necessary to assure state is partly punched, until Oblique vertical position welding and downhand position can use top arc welding;
7th step, it is anti-oxidation, in pipe away from each 100mm in weld bond both sides at, a pair of rubber slab connected with iron wire of setting, plate thickness is 3-5mm is supported inside and outside plate with clamping plate, the metal hose of an a diameter of 3-5mm is filled on one piece of closure plate wherein, is welded Argon filling in Shi Xiangguan after being soldered, is pulled out rubber slab by metal hose;
8th step after the completion of oxidation, using material package weld seam and weld seam both sides are protected, makes weld seam Slow cooling;
9th step cleans groove, then polished smooth with sander after cooling.
The angle of the groove is 20 ° -30 °.
Embodiment one:
A kind of welding method of corrugated conduit, includes the following steps:
The first step, the inspection of pipeline check whether the surface of pipeline has the defects of crackle, shrinkage cavity, folding, pipe;
Second step:Cleaning, cleans pipeline with pipeline cleaning;
Third walks, preheating, and using electric preheating, the heating of uniform stabilization is carried out to bellows;
4th step, groove processing carry out groove processing to bellows;
5th step, polishing, polishes to groove using sander;
6th step, welding, on groove face in striking to gap, makes welding rod make slight lateral swing in two root faces, when root face is molten When changing iron liquid and welding rod molten drop and connecting together, sending on welding rod, electrode tip all reaches groove bottom edge at this time, and the 2/3 of entire electric arc Will be in combustion inner pipe, and first molten hole is formed, when overhead welding is to oblique overhead position arc manipulation, it is necessary to assure state is partly punched, until Oblique vertical position welding and downhand position can use top arc welding;
7th step, it is anti-oxidation, in pipe away from each 100mm in weld bond both sides at, a pair of rubber slab connected with iron wire of setting, plate thickness is 3mm is supported with clamping plate inside and outside plate, fills the metal hose of an a diameter of 3mm on one piece of closure plate wherein, when welding to Argon filling in pipe, after being soldered, is pulled out rubber slab by metal hose;
8th step after the completion of oxidation, using material package weld seam and weld seam both sides are protected, makes weld seam Slow cooling;
9th step cleans groove, then polished smooth with sander after cooling.
The angle of the groove is 20 °.
Embodiment two:
A kind of welding method of corrugated conduit, includes the following steps:
The first step, the inspection of pipeline check whether the surface of pipeline has the defects of crackle, shrinkage cavity, folding, pipe;
Second step:Cleaning, cleans pipeline with pipeline cleaning;
Third walks, preheating, and using electric preheating, the heating of uniform stabilization is carried out to bellows;
4th step, groove processing carry out groove processing to bellows;
5th step, polishing, polishes to groove using sander;
6th step, welding, on groove face in striking to gap, makes welding rod make slight lateral swing in two root faces, when root face is molten When changing iron liquid and welding rod molten drop and connecting together, sending on welding rod, electrode tip all reaches groove bottom edge at this time, and the 2/3 of entire electric arc Will be in combustion inner pipe, and first molten hole is formed, when overhead welding is to oblique overhead position arc manipulation, it is necessary to assure state is partly punched, until Oblique vertical position welding and downhand position can use top arc welding;
7th step, it is anti-oxidation, in pipe away from each 100mm in weld bond both sides at, a pair of rubber slab connected with iron wire of setting, plate thickness is 4mm is supported with clamping plate inside and outside plate, fills the metal hose of an a diameter of 4mm on one piece of closure plate wherein, when welding to Argon filling in pipe, after being soldered, is pulled out rubber slab by metal hose;
8th step after the completion of oxidation, using material package weld seam and weld seam both sides are protected, makes weld seam Slow cooling;
9th step cleans groove, then polished smooth with sander after cooling.
The angle of the groove is 25 °.
Embodiment three:
A kind of welding method of corrugated conduit, includes the following steps:
The first step, the inspection of pipeline check whether the surface of pipeline has the defects of crackle, shrinkage cavity, folding, pipe;
Second step:Cleaning, cleans pipeline with pipeline cleaning;
Third walks, preheating, and using electric preheating, the heating of uniform stabilization is carried out to bellows;
4th step, groove processing carry out groove processing to bellows;
5th step, polishing, polishes to groove using sander;
6th step, welding, on groove face in striking to gap, makes welding rod make slight lateral swing in two root faces, when root face is molten When changing iron liquid and welding rod molten drop and connecting together, sending on welding rod, electrode tip all reaches groove bottom edge at this time, and the 2/3 of entire electric arc Will be in combustion inner pipe, and first molten hole is formed, when overhead welding is to oblique overhead position arc manipulation, it is necessary to assure state is partly punched, until Oblique vertical position welding and downhand position can use top arc welding;
7th step, it is anti-oxidation, in pipe away from each 100mm in weld bond both sides at, a pair of rubber slab connected with iron wire of setting, plate thickness is 5mm is supported with clamping plate inside and outside plate, fills the metal hose of an a diameter of 5mm on one piece of closure plate wherein, when welding to Argon filling in pipe, after being soldered, is pulled out rubber slab by metal hose;
8th step after the completion of oxidation, using material package weld seam and weld seam both sides are protected, makes weld seam Slow cooling;
9th step cleans groove, then polished smooth with sander after cooling.
The angle of the groove is 30 °.
The embodiments of the present invention have been described in detail above, but content is only the preferred embodiment of the present invention, Should not be construed as limiting the present invention practical range, any changes and modifications in accordance with the scope of the present application, It should all still fall within the scope of the patent of the present invention.

Claims (2)

1. a kind of welding method of corrugated conduit, it is characterised in that:Include the following steps:
The first step, the inspection of pipeline check whether the surface of pipeline has the defects of crackle, shrinkage cavity, folding, pipe;
Second step:Cleaning, cleans pipeline with pipeline cleaning;
Third walks, preheating, and using electric preheating, the heating of uniform stabilization is carried out to bellows;
4th step, groove processing carry out groove processing to bellows;
5th step, polishing, polishes to groove using sander;
6th step, welding, on groove face in striking to gap, makes welding rod make slight lateral swing in two root faces, when root face is molten When changing iron liquid and welding rod molten drop and connecting together, sending on welding rod, electrode tip all reaches groove bottom edge at this time, and the 2/3 of entire electric arc Will be in combustion inner pipe, and first molten hole is formed, when overhead welding is to oblique overhead position arc manipulation, it is necessary to assure state is partly punched, until Oblique vertical position welding and downhand position can use top arc welding;
7th step, it is anti-oxidation, in pipe away from each 100mm in weld bond both sides at, a pair of rubber slab connected with iron wire of setting, plate thickness is 3-5mm is supported inside and outside plate with clamping plate, the metal hose of an a diameter of 3-5mm is filled on one piece of closure plate wherein, is welded Argon filling in Shi Xiangguan after being soldered, is pulled out rubber slab by metal hose;
8th step after the completion of oxidation, using material package weld seam and weld seam both sides are protected, makes weld seam Slow cooling;
9th step cleans groove, then polished smooth with sander after cooling.
2. a kind of welding method of corrugated conduit according to claim 1, it is characterised in that:The angle of the groove is 20°-30°。
CN201810370844.3A 2018-04-24 2018-04-24 A kind of welding method of corrugated conduit Pending CN108568582A (en)