CN108086027A - A kind of methods of beating for improving softwood pulp beating degree - Google Patents

A kind of methods of beating for improving softwood pulp beating degree Download PDF

Info

Publication number
CN108086027A
CN108086027A CN201711309902.3A CN201711309902A CN108086027A CN 108086027 A CN108086027 A CN 108086027A CN 201711309902 A CN201711309902 A CN 201711309902A CN 108086027 A CN108086027 A CN 108086027A
Authority
CN
China
Prior art keywords
beating
parts
improving
methods
softwood pulp
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CN201711309902.3A
Other languages
Chinese (zh)
Inventor
许亦南
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
ANHUI BILUN LIVING PAPER Co Ltd
Original Assignee
ANHUI BILUN LIVING PAPER Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by ANHUI BILUN LIVING PAPER Co Ltd filed Critical ANHUI BILUN LIVING PAPER Co Ltd
Priority to CN201711309902.3A priority Critical patent/CN108086027A/en
Publication of CN108086027A publication Critical patent/CN108086027A/en
Pending legal-status Critical Current

Abstract

The invention belongs to paper for daily use technical fields, and in particular to a kind of methods of beating for improving softwood pulp beating degree including needlebush pulpboard is discongested with hydrabrusher, with treatment fluid isothermal holding, is then coordinated with abrasive and is beaten.The present invention has the following advantages compared with prior art:Material discongests needlebush pulpboard by treatment fluid in the present invention and carries out high temperature immersion treatment, fiber profit can be made to rise, generate fiber fines or fibrous refinement, destroy fibre structure, the active ingredient for the treatment of fluid can enter fibrous inside, fibrous inside is made to form amorphous region, weaken the combination of fiber quality inspection, then the use of abrasive is coordinated again, can be further fiber surface activation and relaxation, under mechanicals efforts, fiber can easier be cut off and wire-dividing broom purification, contributes to the raising of needlebush beating degree.

Description

A kind of methods of beating for improving softwood pulp beating degree
Technical field
The invention belongs to paper for daily use technical fields, and in particular to a kind of methods of beating for improving softwood pulp beating degree.
Background technology
Paper for daily use develops rapidly in recent years, and toilet paper portion is also increasing, and relevant expert is appealing to prevent While toilet paper excess capacity, the production cost problem of concern toilet paper is also begun to, in order to reduce the production cost of factory, together The productivity effect of Shi Tigao factories, more and more paper mills pre-process slurry with biological enzyme in pulping process, Slurry is copied into that various physical properties after paper are unalterable while reduce the energy consumption in pulping process, although toilet paper Raw material multiselect hardwood pulp, but also have a small number of products and can add some softwood pulps to improve quality, due to needlebush The beating degree of slurry is difficult to improve, and using biological enzyme auxiliary mashing in existing method, but it is unsatisfactory to promote effect.
The content of the invention
The purpose of the present invention is being directed to the problem of existing, a kind of methods of beating for improving softwood pulp beating degree is provided.
The present invention is achieved by the following technical solutions:A kind of methods of beating for improving softwood pulp beating degree, including Following steps:
(1)Treatment fluid is prepared:By weight, 3-5 parts of light-coloured vinegar, 1.3-1.7 parts of hydrogen peroxide, persimmon leaf extract 0.8- are taken 1.2 parts, 0.3-0.5 parts of Conyza japonica extract, 100 parts of water are mixed to get treatment fluid;
(2)Abrasive is prepared:By weight, including 12-18 parts of nano-sized carbon, 5-7 parts of nano-calcium carbonate, 2-4 parts of Nanometer Copper;
(3)Needlebush pulpboard is discongested with hydrabrusher, the treatment fluid heat-insulation soaking 3- for being then 85-95 DEG C with temperature 4 it is small when, obtain impregnate material it is spare;
(4)The abrasive for being equivalent to its weight 3-6% is added in above-mentioned spare immersion material, is beaten with PFI fiberizers.
As further improvement of these options, the main component of the persimmon leaf extract is natural Victoria C, rutin, Choline, glycosides displayed;The Conyza japonica extract is the extract of Conyza japonica aerial part, and main component is rigidness formic acid, effectively The content of ingredient is 1%;The persimmon leaf extract and Conyza japonica extract Jun Youxianchang high mountains bio tech ltd provide.
As further improvement of these options, the grain size of the nano-sized carbon is 400-800nm;The nano-calcium carbonate Grain size be 400-2000nm;The grain size of the Nanometer Copper is 20-100nm.
As further improvement of these options, the step(3)With 200-400 revs/min of rotating speed in soaking process Clock stirs.
As further improvement of these options, the step(4)It is middle to control beating degree as 30 ° of SR, control slurry trip It is 340-360mL from degree.
The present invention has the following advantages compared with prior art:By treatment fluid needlebush pulpboard is discongested in the present invention expect into Row high temperature immersion treatment can make fiber profit rise, generate fiber fines or fibrous refinement, destroy fibre structure, and treatment fluid has Fibrous inside can be entered by imitating ingredient, and fibrous inside is made to form amorphous region, weakens the combination of fiber quality inspection, then coordinates grinding again The use of material, can be further fiber surface activation and relaxation, under mechanicals efforts, fiber can easier cut off and Wire-dividing broom purification contributes to the raising of needlebush beating degree.
Specific embodiment
Embodiment 1
A kind of methods of beating for improving softwood pulp beating degree, comprises the following steps:
(1)Treatment fluid is prepared:By weight, 4 parts of light-coloured vinegar, 1.5 parts of hydrogen peroxide, 1 part of persimmon leaf extract, Conyza japonica is taken to carry 0.4 part of object is taken, 100 parts of water is mixed to get treatment fluid;
(2)Abrasive is prepared:By weight, including 15 parts of nano-sized carbon, 6 parts of nano-calcium carbonate, 3 parts of Nanometer Copper;
(3)Needlebush pulpboard is discongested with hydrabrusher, it is then small with treatment fluid heat-insulation soaking 3.5 at a temperature of 90 °C When, it is spare to obtain immersion material;
(4)The abrasive for being equivalent to its weight 4.5% is added in above-mentioned spare immersion material, is beaten with PFI fiberizers.
Wherein, the main component of the persimmon leaf extract is natural Victoria C, rutin, choline, glycosides displayed;The Conyza japonica Extract is the extract of Conyza japonica aerial part, and main component is rigidness formic acid, and the content of active ingredient is 1%;The persimmon Leaf extract and Conyza japonica extract Jun Youxianchang high mountains bio tech ltd provide;The grain size of the nano-sized carbon is 400- 800nm;The grain size of the nano-calcium carbonate is 400-2000nm;The grain size of the Nanometer Copper is 20-100nm.
Wherein, the step(3)With 300 revs/min of stirrings of rotating speed in soaking process;The step(4)Middle control is beaten The degree of beating is 30 ° of SR, and it is 350mL to control stock freeness.
Embodiment 2
A kind of methods of beating for improving softwood pulp beating degree, comprises the following steps:
(1)Treatment fluid is prepared:By weight, 3 parts of light-coloured vinegar, 1.3 parts of hydrogen peroxide, 0.8 part of persimmon leaf extract, Conyza japonica are taken 0.3 part of extract, 100 parts of water, is mixed to get treatment fluid;
(2)Abrasive is prepared:By weight, including 12 parts of nano-sized carbon, 7 parts of nano-calcium carbonate, 2 parts of Nanometer Copper;
(3)Needlebush pulpboard is discongested with hydrabrusher, it is then small with the treatment fluid heat-insulation soaking 4 that temperature is 85 DEG C When, it is spare to obtain immersion material;
(4)The abrasive for being equivalent to its weight 3% is added in above-mentioned spare immersion material, is beaten with PFI fiberizers.
Wherein, the main component of the persimmon leaf extract is natural Victoria C, rutin, choline, glycosides displayed;The Conyza japonica Extract is the extract of Conyza japonica aerial part, and main component is rigidness formic acid, and the content of active ingredient is 1%;The persimmon Leaf extract and Conyza japonica extract Jun Youxianchang high mountains bio tech ltd provide;The grain size of the nano-sized carbon is 400- 800nm;The grain size of the nano-calcium carbonate is 400-2000nm;The grain size of the Nanometer Copper is 20-100nm.
Wherein, the step(3)With 400 revs/min of stirrings of rotating speed in soaking process;The step(4)Middle control is beaten The degree of beating is 30 ° of SR, and it is 340mL to control stock freeness.
Embodiment 3
A kind of methods of beating for improving softwood pulp beating degree, comprises the following steps:
(1)Treatment fluid is prepared:By weight, 5 parts of light-coloured vinegar, 1.7 parts of hydrogen peroxide, 1.2 parts of persimmon leaf extract, Conyza japonica are taken 0.5 part of extract, 100 parts of water, is mixed to get treatment fluid;
(2)Abrasive is prepared:By weight, including 18 parts of nano-sized carbon, 5 parts of nano-calcium carbonate, 4 parts of Nanometer Copper;
(3)Needlebush pulpboard is discongested with hydrabrusher, it is then small with the treatment fluid heat-insulation soaking 3 that temperature is 95 DEG C When, it is spare to obtain immersion material;
(4)The abrasive for being equivalent to its weight 6% is added in above-mentioned spare immersion material, is beaten with PFI fiberizers.
Wherein, the main component of the persimmon leaf extract is natural Victoria C, rutin, choline, glycosides displayed;The Conyza japonica Extract is the extract of Conyza japonica aerial part, and main component is rigidness formic acid, and the content of active ingredient is 1%;The persimmon Leaf extract and Conyza japonica extract Jun Youxianchang high mountains bio tech ltd provide;The grain size of the nano-sized carbon is 400- 800nm;The grain size of the nano-calcium carbonate is 400-2000nm;The grain size of the Nanometer Copper is 20-100nm.
Wherein, the step(3)With 200 revs/min of stirrings of rotating speed in soaking process;The step(4)Middle control is beaten The degree of beating is 30 ° of SR, and it is 360mL to control stock freeness.
Control group 1 is set, by step in embodiment 1(1)And its removed using step, remaining content is constant;Control is set Group 2, by step in embodiment 1(2)And its removed using step, remaining content is constant;Control group 3 is set, by step(3)Processing Material of discongesting afterwards is handled with cellulase solution, and cellulase solution concentration is 0.20IU/g, then defibrination according to a conventional method;
Detection each group PFI mills are meeting revolution of the beating degree for 30 ° of SR, and cake, which is pressed, quantifies 60g/m2 handsheets, and every group is manufactured paper with pulp 5, is done Dry, equilibrium water conten, detection physical property obtains following result:
Table 1
Group PFI grinds revolution Tear index(mN·m²/g) Burst index
Embodiment 1 1900 14.694 3.172
Embodiment 2 1950 14.685 3.168
Embodiment 3 1900 14.687 3.169
Control group 1 2800 10.735 2.746
Control group 2 2700 12.816 2.853
Control group 3 2300 14.685 3.147
The defibrination degree for compared with prior art, reaching identical is can be seen that in the present invention by data in table 1, can reduce PFI mills Revolution reduces energy consumption, and products obtained therefrom comprehensive performance can reach preferable level, suitable for promoting the use of.

Claims (5)

1. a kind of methods of beating for improving softwood pulp beating degree, which is characterized in that comprise the following steps:
(1)Treatment fluid is prepared:By weight, 3-5 parts of light-coloured vinegar, 1.3-1.7 parts of hydrogen peroxide, persimmon leaf extract 0.8- are taken 1.2 parts, 0.3-0.5 parts of Conyza japonica extract, 100 parts of water are mixed to get treatment fluid;
(2)Abrasive is prepared:By weight, including 12-18 parts of nano-sized carbon, 5-7 parts of nano-calcium carbonate, 2-4 parts of Nanometer Copper;
(3)Needlebush pulpboard is discongested with hydrabrusher, the treatment fluid heat-insulation soaking 3- for being then 85-95 DEG C with temperature 4 it is small when, obtain impregnate material it is spare;
(4)The abrasive for being equivalent to its weight 3-6% is added in above-mentioned spare immersion material, is beaten with PFI fiberizers.
2. a kind of methods of beating for improving softwood pulp beating degree as described in claim 1, which is characterized in that the persimmon leaves carry The main component of object is taken as natural Victoria C, rutin, choline, glycosides displayed;The Conyza japonica extract carries for Conyza japonica aerial part Object is taken, main component is rigidness formic acid, and the content of active ingredient is 1%;The persimmon leaf extract and Conyza japonica extract have Xian Chang high mountains bio tech ltd provides.
3. a kind of methods of beating for improving softwood pulp beating degree as described in claim 1, which is characterized in that the nano-sized carbon Grain size is 400-800nm;The grain size of the nano-calcium carbonate is 400-2000nm;The grain size of the Nanometer Copper is 20-100nm.
A kind of 4. methods of beating for improving softwood pulp beating degree as described in claim 1, which is characterized in that the step(3) With 200-400 revs/min of stirring of rotating speed in soaking process.
A kind of 5. methods of beating for improving softwood pulp beating degree as described in claim 1, which is characterized in that the step(4) Middle to control beating degree as 30 ° of SR, it is 340-360mL to control stock freeness.
CN201711309902.3A 2017-12-11 2017-12-11 A kind of methods of beating for improving softwood pulp beating degree Pending CN108086027A (en)