CN106759502A - A kind of manufacture method of antirust walling crib - Google Patents

A kind of manufacture method of antirust walling crib Download PDF

Info

Publication number
CN106759502A
CN106759502A CN201610930433.6A CN201610930433A CN106759502A CN 106759502 A CN106759502 A CN 106759502A CN 201610930433 A CN201610930433 A CN 201610930433A CN 106759502 A CN106759502 A CN 106759502A
Authority
CN
China
Prior art keywords
walling crib
antirust
manufacture method
well lid
blank
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CN201610930433.6A
Other languages
Chinese (zh)
Inventor
王建辉
王荣跃
李春福
酉治洪
徐伟
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Sichuan Yi Cheng Technology Co Ltd
Original Assignee
Sichuan Yi Cheng Technology Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Sichuan Yi Cheng Technology Co Ltd filed Critical Sichuan Yi Cheng Technology Co Ltd
Priority to CN201610930433.6A priority Critical patent/CN106759502A/en
Publication of CN106759502A publication Critical patent/CN106759502A/en
Pending legal-status Critical Current

Abstract

The invention discloses a kind of manufacture method of antirust walling crib, the manufacture method of walling crib that this is antirust is comprised the following steps:Sorting, solution treatment, kerve, interior endless tube, polishing, manufacture walling crib, the step such as spraying of wearable coating are inserted, by processing technology reliability, realize the antifreeze treatment of walling crib, overall structure is more reliable.

Description

A kind of manufacture method of antirust walling crib
Technical field
The present invention relates to well hole auxiliary device field, specifically a kind of manufacture method of antirust walling crib.
Background technology
Currently, with the development of the city and road reformation, a large amount of communication, power cables for setting on the ground etc. are required for Underground is moved on to, is re-started and is laid.These facilities are safeguarded and changed in the future for convenience.So being accomplished by building a large amount of Inspection shaft meet engineering maintenance in the future and the need for maintenance is changed.The appearance of these inspection shafts, really to maintenance in the future and Maintenance is changed to provide and greatly facilitated.But in the winter time, the particularly more cold area of weather, under Snowfall, well lid Junction with walling crib easily freezes, when run into line fault need open well lid overhauled when, in addition it is also necessary to ice sheet is smashed to pieces, Ability breakdown well lid, if ice sheet is thicker, the ice sheet covered on well lid is thicker, is difficult to smash to pieces, and overexerts, it is also possible to cause Well lid Integral-crushing.
The content of the invention
The present invention is intended to provide a kind of manufacture method of antirust walling crib, to solve the above problems.
To achieve the above object, technical scheme is as follows:
A kind of manufacture method of antirust walling crib, it is characterised in that comprise the following steps:
Sorting:From 304 stainless steel materials as blank, Size calculation is carried out according to well lid size, then use cutting machine according to Target size after calculating cuts blank;
Solution treatment:Solution treatment will be carried out with the pipe after treatment, 1050 DEG C of keeping temperature, 15 minutes duration, then Quick cooling;
Kerve:Blank after polishing is warming up to 550 DEG C ~ 650 DEG C, first time hot-drawn groove is carried out, entered again after first time Hot drawing The above-mentioned solutionizing step of row, then blank is placed in mould carries out second hot-drawn groove;
Insert interior endless tube:Well lid circumference is placed in from endless tube, and carbon fiber heating silk is laid in endless tube;
Polishing:Surface polishing is carried out, sanding burr totally and is polished;
Manufacture walling crib:50 ~ 80 parts of cement, 3 ~ 5 parts of lime, 8 ~ 20 parts of wollastonites, 1 part of water-cement ratio, 25 ~ 50 parts of sandstones are mixed and is stirred Concrete mix is mixed, is added in outer walling crib mould and carries out outer walling crib forming processes;
Basecoat paint:To walling crib and well lid surface spraying/roller coating prime paint, and dry 30 minutes;
Surface lacquer is sprayed:In prime paint surface laser spraying of wearable coating, after drying 0.5-1.5 hours, spraying three times is repeated.
Further, the wear-resistant coating thickness is 100 μm -120 μm.
Further, seal mortar treatent is done in the endless tube, and in well lid bottom metal material reinforcement.
Further, the reinforcement is crisscross setting.
Further, the reinforcement includes four horizontal bars and three perpendicular muscle.
The beneficial effects of the present invention are:Using 304 stainless steels, can effectively anticorrosive oxidation, it is to avoid well lid is in specific ring The problem that service life shortens in border, in more cold winter, powers by carbon fiber wire, can convert electric energy to heat Can, it is to avoid well lid and interior walling crib junction produce and the phenomenon such as freeze and cause the well lid cannot to open.
Specific embodiment
With reference to specific embodiment, the present invention will be further described.
A kind of manufacture method of antirust walling crib, it is characterised in that comprise the following steps:
Sorting:From 304 stainless steel materials as blank, Size calculation is carried out according to well lid size, then use cutting machine according to Target size after calculating cuts blank;
Solution treatment:Solution treatment will be carried out with the pipe after treatment, 1050 DEG C of keeping temperature, 15 minutes duration, then Quick cooling;
Kerve:Blank after polishing is warming up to 550 DEG C ~ 650 DEG C, first time hot-drawn groove is carried out, entered again after first time Hot drawing The above-mentioned solutionizing step of row, then blank is placed in mould carries out second hot-drawn groove;
Insert interior endless tube:Well lid circumference is placed in from endless tube, and carbon fiber heating silk is laid in endless tube;
Polishing:Surface polishing is carried out, sanding burr totally and is polished;
Manufacture walling crib:50 ~ 80 parts of cement, 3 ~ 5 parts of lime, 8 ~ 20 parts of wollastonites, 1 part of water-cement ratio, 25 ~ 50 parts of sandstones are mixed and is stirred Concrete mix is mixed, is added in outer walling crib mould and carries out outer walling crib forming processes;
Basecoat paint:To walling crib and well lid surface spraying/roller coating prime paint, and dry 30 minutes;
Surface lacquer is sprayed:In prime paint surface laser spraying of wearable coating, after drying 0.5-1.5 hours, spraying three times is repeated.
The wear-resistant coating thickness is 100 μm -120 μm.
Seal mortar treatent is done in the endless tube, and in well lid bottom metal material reinforcement.
The reinforcement is crisscross setting.
The reinforcement includes four horizontal bars and three perpendicular muscle.
Using 304 stainless steels, can effectively anticorrosive oxidation, it is to avoid well lid asking of shortening of service life in specific environment Topic, in more cold winter, powers by carbon fiber wire, can convert electric energy to heat energy, it is to avoid well lid and interior walling crib Junction produces and the phenomenon such as freezes and cause the well lid cannot to open.
The preferred embodiments of the present invention are the foregoing is only, is not intended to limit the invention, for the skill of this area For art personnel, the present invention can have various modifications and variations.It is all within the spirit and principles in the present invention, made any repair Change, equivalent, improvement etc., should be included within the scope of the present invention.

Claims (5)

1. a kind of manufacture method of antirust walling crib, it is characterised in that comprise the following steps:
Sorting:From 304 stainless steel materials as blank, Size calculation is carried out according to well lid size, then use cutting machine according to Target size after calculating cuts blank;
Solution treatment:Solution treatment will be carried out with the pipe after treatment, 1050 DEG C of keeping temperature, 15 minutes duration, then Quick cooling;
Kerve:Blank after polishing is warming up to 550 DEG C ~ 650 DEG C, first time hot-drawn groove is carried out, entered again after first time Hot drawing The above-mentioned solutionizing step of row, then blank is placed in mould carries out second hot-drawn groove;
Insert interior endless tube:Well lid circumference is placed in from endless tube, and carbon fiber heating silk is laid in endless tube;
Polishing:Surface polishing is carried out, sanding burr totally and is polished;
Manufacture walling crib:50 ~ 80 parts of cement, 3 ~ 5 parts of lime, 8 ~ 20 parts of wollastonites, 1 part of water-cement ratio, 25 ~ 50 parts of sandstones are mixed and is stirred Concrete mix is mixed, is added in outer walling crib mould and carries out outer walling crib forming processes;
Basecoat paint:To walling crib and well lid surface spraying/roller coating prime paint, and dry 30 minutes;
Surface lacquer is sprayed:In prime paint surface laser spraying of wearable coating, after drying 0.5-1.5 hours, spraying three times is repeated.
2. the manufacture method of antirust walling crib according to claim 1, it is characterised in that the wear-resistant coating thickness is 100 μ m-120μm。
3. the manufacture method of antirust walling crib according to claim 1, it is characterised in that do seal mortar treatent in the endless tube, And in well lid bottom metal material reinforcement.
4. the manufacture method of antirust walling crib according to claim 3, it is characterised in that the reinforcement sets for crisscross Put.
5. the manufacture method of antirust walling crib according to claim 4, it is characterised in that the reinforcement includes four horizontal bars With three perpendicular muscle.
CN201610930433.6A 2016-10-31 2016-10-31 A kind of manufacture method of antirust walling crib Pending CN106759502A (en)