CN106423581A - Lead-antimony-zinc sulfide ore bulk flotation collecting agent and preparation and application thereof - Google Patents
Lead-antimony-zinc sulfide ore bulk flotation collecting agent and preparation and application thereof Download PDFInfo
- Publication number
- CN106423581A CN106423581A CN201611003897.9A CN201611003897A CN106423581A CN 106423581 A CN106423581 A CN 106423581A CN 201611003897 A CN201611003897 A CN 201611003897A CN 106423581 A CN106423581 A CN 106423581A
- Authority
- CN
- China
- Prior art keywords
- agent
- collecting agent
- bulk flotation
- kerosene
- lead
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Granted
Abstract
The invention relates to a lead-antimony-zinc sulfide ore bulk flotation collecting agent and preparation and application thereof. The gearbox left box body shell is prepared by mixing tert-dodecyl mercaptan and emulsified kerosene. The mass ratio of the tert-dodecyl mercaptan to the emulsified kerosene is 1:(0.9-1.2). The lead-antimony-zinc sulfide ore bulk flotation collecting agent has the better collecting effect on sulfide, and can be applied to lead-antimony-zinc sulfide ore bulk flotation. The lead-antimony-zinc sulfide ore bulk flotation collecting agent has the good foaming property, can adopt a small amount or no foaming agent, and can decrease the consumption of an activating agent copper sulfate; compared with traditional MA or single use of emulsified kerosene and tert-dodecyl mercaptan, the grade and recycling rate of sulfide can be increased, and types and consumption of medicament are reduced.
Description
Technical field
The present invention relates to a kind of lead antimony zinc vulcanizing mine bulk flotation collecting agent, belong to mineral working process technical field.
Background technology
Guanxi Nandan Che He ore dressing plant, its ore field is the lead antimony zinc multi-metal sulfide mineral deposit based on cassiterite, its master
Mineral to be processed have cassiterite, jamesonite, marmatite, magnetic iron ore, pyrite, main recovery:Cassiterite, lead antimony and
Zinc.The flow process of employing is at present:Gravity-floatation re-selection procedure, in flotation part using heavy dose of collecting agent, activator
Remove sulphide ore with foaming agent, be that rear gravity treatment cassiterite creates conditions, wherein, collecting agent is MA, and activator is copper sulphate, foaming agent
For No. two oil.
Because dosing is big, and ore chats species are various, and paragenetic association is complicated, do not only exist environment at present dirty
Dye, the problems such as the rate of recovery is unstable, and causes adverse effect to the separating treatment of follow-up sulphide ore.In order to improve the rate of recovery and
Reduce the difficulty of subsequent treatment, the exploitation of related agents is all paid attention to by full factory always.
Content of the invention
For the defect of prior art, the purpose of the present invention is to be to provide a kind of lead antimony zinc vulcanizing mine bulk flotation collecting
Agent, to improve grade and the rate of recovery, minimizing medicament kind and the consumption of sulfide.
The technical scheme is that:A kind of lead antimony zinc vulcanizing mine bulk flotation collecting agent, by tert-dodecyl mercaptan and emulsification
Kerosene is mixed, and tert-dodecyl mercaptan and emulsified kerosene mass ratio are 1:(0.9~1.2).
In a detailed embodiment, described emulsified kerosene is in mass ratio the 1 of emulsifying agent, kerosene and water:12~17:
70 ~ 75 mixing, make through ultrasonic emulsification.
In a detailed embodiment, described emulsifying agent is Tween-20 and/or PEG-400.
In a detailed embodiment, by tert-dodecyl mercaptan and emulsified kerosene in mass ratio 1:(0.9 ~ 1.2), ultrasonic shake
Swing mix prepared.
In a detailed embodiment, during ultrasonic vibration mixing, ultrasonic frequency is 20 ~ 40kHz, and incorporation time is 20
~30min.
In a detailed embodiment, described emulsified kerosene be made of emulsifying agent, kerosene and water through ultrasonic emulsification, surpass
Frequency of sound wave is 20 ~ 40kHz, and when emulsifying agent adopts Tween-20 or PEG-400, emulsification times are 60 ~ 80min, and emulsifying agent adopts
When Tween-20 and PEG-400, phaco time is 40 ~ 50min.
The present invention also provides a kind of application in lead antimony zinc vulcanizing mine bulk flotation for described collecting agent, and regime of agent is thick
Copper sulphate 25 ~ 35 g/t, described collecting agent 15 ~ 25 g/t when selecting, described collecting agent 8 ~ 12 g/t when scanning, the ore pulp of flotation is not
PH regulator need to be added, using nature pH, be not added with foaming agent.
With respect to prior art, the hybrid collector for lead antimony zinc vulcanizing mine flotation of the present invention has advantages below:
1)This hybrid collector good stability, at room temperature can be with emulsion form stable existence 60min, emulsion drop after adding water
d50Being basically unchanged, stably can play a role within the flotation of ore pulp time;
2)This hybrid collector is strong in the dispersibility of ore pulp, with mineral effect fully, improves floatation indicators obvious;
3)This hybrid collector foaming characteristic is good, and foam is tiny, uniform, can reduce foaming agent and use, or can replace foaming agent;
4)This hybrid collector(To be calculated with emulsified kerosene quality summation with actual tert-dodecyl mercaptan)Subtract with frother dosages
Few, reduce reagent cost.
The hybrid collector of the present invention has preferable collecting effect to sulfide, can apply to lead antimony zinc vulcanizing mine and floats
Choosing.It has good foaming characteristic, can add less or be not added with foaming agent, can reduce the consumption of activator copper sulphate.Compare simultaneously
Traditional MA, it is used alone tert-dodecyl mercaptan and emulsified kerosene, grade and the rate of recovery of sulfide can be improved, decrease medicament
Species and consumption.
Specific embodiment
Following examples are intended to further illustrate present invention, but protection scope of the present invention is not subject to these embodiments
Limit.
Preparation embodiment 1
1)The preparation of emulsified kerosene:Emulsifying agent(Tween-20 and PEG-400 mass ratio 1:1 mixture), kerosene and water by matter
Amount compares 1:15:70 mixing, ultrasonic frequency is 20 ~ 40kHz, through ultrasonic emulsification 40 ~ 50min;
2)By tert-dodecyl mercaptan(Purity is higher than 95%)With step 1)The emulsified kerosene of preparation is 1 in mass ratio:1 mixing, using super
Acoustic shock is swung makes it fully mix, and ultrasonic frequency is 20 ~ 40kHz, and incorporation time is 20 ~ 30min, is prepared into hybrid collector.
The hybrid collector made at room temperature can be with emulsion form stable existence 60min, emulsion drop d after adding water50
Being basically unchanged;Foaming characteristic is good, and foam is tiny, uniform.
Application Example 1
In Dachang, Guangxi 92# ore body ore, sulfide mineral includes, jamesonite, marmatite, magnetic iron ore and pyrite, when
When raw ore contains Pb 0.248%, contains Sb 0.192%, contains Zn 2.128%, account for 80.32% in raw ore mog for -200 mesh
In the case of, using one roughing, triple cleaning, the flotation flowsheet of once purging selection, regime of agent is roughly selected using copper sulphate 30 g/t,
Hybrid collector 20 g/t that preparation embodiment 1 provides, scans hybrid collector 10 g/t using preparation embodiment 1, selected
Selected using blank, closed circuit experiment is carried out using above-mentioned flow process and regime of agent, sulphide ore bulk concentrate may finally be obtained and contain
Pb 1.781%, Zn 15.458%, Sb 1.354%, the Pb rate of recovery 93.688%, the Zn rate of recovery 94.768%, the Sb rate of recovery
91.859% excellent measure.
Comparative example 1
The collecting agent that this comparative example adopts is single emulsified kerosene, sulfide mineral bag in Dachang, Guangxi 92# ore body ore
Include, jamesonite, marmatite, magnetic iron ore and pyrite, when raw ore contains Pb 0.244%, contains Sb 0.194%, contains Zn
When 2.141%, in the case of raw ore mog accounts for 79.86% for -200 mesh, using one roughing, triple cleaning, once sweep
The flotation flowsheet of choosing, regime of agent is roughly selected using activator copper sulphate 80 g/t, collecting agent emulsified kerosene 200 g/t, foaming agent
2# oil 40g/t;Scan using collecting agent emulsified kerosene 100 g/t, foaming agent 2# oil 20g/t;Selected selected using blank, adopt
Above-mentioned flow process and regime of agent carry out closed circuit experiment, may finally obtain sulphide ore bulk concentrate and contain Pb 1.401%, Zn
12.109%, Sb 1.120%, the Pb rate of recovery 88.206%, the Zn rate of recovery 86.875%, the index of the Sb rate of recovery 89.649%.
Comparative example 2
The collecting agent that this comparative example adopts is single tert-dodecyl mercaptan.Sulfide mineral in Dachang, Guangxi 92# ore body ore
Including jamesonite, marmatite, magnetic iron ore and pyrite, when raw ore contains Pb 0.246%, contains Sb 0.203%, contains
During Zn 2.139%, in the case of raw ore mog accounts for 79.86% for -200 mesh, using one roughing, triple cleaning, once
The flotation flowsheet scanned, regime of agent is roughly selected using activator copper sulphate 80 g/t, collecting agent tert-dodecyl mercaptan 200 g/t, rises
Infusion 2# oil 40g/t;Scan using collecting agent tert-dodecyl mercaptan 100 g/t, foaming agent 2# oil 20g/t;Selected smart using blank
Choosing, carries out closed circuit experiment using above-mentioned flow process and regime of agent, may finally obtain sulphide ore bulk concentrate and contain Pb 1.431%,
Zn 12.268%, Sb 1.195%, the Pb rate of recovery 89.350%, the Zn rate of recovery 88.096%, the index of the Sb rate of recovery 90.420%.
By Application Example 1 and comparative example 1 ~ 2 as can be seen that lead antimony zinc sulphur is used for using the collecting agent of the present invention
Change ore deposit bulk flotation, tert-dodecyl mercaptan and emulsified kerosene Synergistic.Cannot be contemplated that uncle 12 sulphur from comparative example 1 ~ 2
Alcohol and emulsified kerosene as proportions of the present invention and greatly reduce consumption and can reach indicated by the indices of Application Example 1
Effect.
Comparative example 3
The collecting agent that this comparative example adopts be scene with medicament MA xanthate, the flow process of employing is scene thick with flow process one
Two sweep three essences.In Dachang, Guangxi 92# ore body ore, sulfide mineral includes, jamesonite, marmatite, magnetic iron ore and Huang Tie
Ore deposit, when raw ore contains Pb 0.244%, contains Sb 0.197%, contains Zn 2.141%, accounts for for -200 mesh in raw ore mog
In the case of 81.23%, using one roughing, triple cleaning, the flotation flowsheet scanned twice, regime of agent is roughly selected and is adopted activator
Copper sulphate 80 g/t, collecting agent MA xanthate 200 g/t, foaming agent 2# oil 40g/t;Scan one and adopt collecting agent MA xanthate 80 g/
T, foaming agent 2# oil 20g/t;Scan two and adopt collecting agent MA xanthate 20 g/t, foaming agent 2# oil 10g/t;Selected smart using blank
Choosing, carries out closed circuit experiment using above-mentioned flow process and regime of agent, may finally obtain sulphide ore bulk concentrate and contain Pb 1.311%,
Zn 11.178%, Sb 1.032%, the Pb rate of recovery 85.884%, the Zn rate of recovery 83.481%, the index of the Sb rate of recovery 83.795%.
Claims (7)
1. a kind of lead antimony zinc vulcanizing mine bulk flotation collecting agent it is characterised in that:System is mixed by tert-dodecyl mercaptan with emulsified kerosene
Become, tert-dodecyl mercaptan and emulsified kerosene mass ratio are 1:(0.9~1.2).
2. lead antimony zinc vulcanizing mine bulk flotation collecting agent according to claim 1 it is characterised in that:Described emulsified kerosene is
In mass ratio the 1 of emulsifying agent, kerosene and water:12~17:70 ~ 75 mixing, make through ultrasonic emulsification.
3. lead antimony zinc vulcanizing mine bulk flotation collecting agent according to claim 2 it is characterised in that:Described emulsifying agent is to tell
Temperature -20 and/or PEG-400.
4. a kind of preparation method of lead antimony zinc vulcanizing mine bulk flotation collecting agent it is characterised in that:By tert-dodecyl mercaptan and emulsification
Kerosene in mass ratio 1:(0.9 ~ 1.2), ultrasonic vibration mixes prepared.
5. according to claim 4 lead antimony zinc vulcanizing mine bulk flotation collecting agent preparation method it is characterised in that:Ultrasonic shake
When swinging mixing, ultrasonic frequency is 20 ~ 40kHz, and incorporation time is 20 ~ 30min.
6. according to claim 4 lead antimony zinc vulcanizing mine bulk flotation collecting agent preparation method it is characterised in that:Described breast
Changing kerosene is made of emulsifying agent, kerosene and water through ultrasonic emulsification, and ultrasonic frequency is 20 ~ 40kHz, emulsifying agent adopt tween-
When 20 or PEG-400, emulsification times are 60 ~ 80min, emulsifying agent adopt Tween-20 and during PEG-400 phaco time be 40 ~
50min.
7. application in lead antimony zinc vulcanizing mine bulk flotation for the described collecting agent of one of a kind of claim 1 ~ 3, its feature exists
In:Regime of agent is copper sulphate 25 ~ 35 g/t, described collecting agent 15 ~ 25 g/t when roughly selecting, described collecting agent 8 ~ 12 when scanning
G/t, the ore pulp of flotation is not required to add pH regulator, using nature pH, is not added with foaming agent.