CN106398242A - Method of producing high-performance modified asphalt by utilizing mineral powder recovered by asphalt mixing station as well as pyrolytic oil and rubber powder of waste tyre and product of method - Google Patents
Method of producing high-performance modified asphalt by utilizing mineral powder recovered by asphalt mixing station as well as pyrolytic oil and rubber powder of waste tyre and product of method Download PDFInfo
- Publication number
- CN106398242A CN106398242A CN201610772623.XA CN201610772623A CN106398242A CN 106398242 A CN106398242 A CN 106398242A CN 201610772623 A CN201610772623 A CN 201610772623A CN 106398242 A CN106398242 A CN 106398242A
- Authority
- CN
- China
- Prior art keywords
- asphalt
- performance modified
- rubber
- breeze
- waste tyre
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Granted
Abstract
The invention discloses a method of producing high-performance modified asphalt by utilizing mineral powder recovered by an asphalt mixing station as well as pyrolytic oil and rubber powder of a waste tyre and a product of the method. The high-performance modified asphalt is prepared from the following components in percentage by weight: 40-50 percent of petroleum asphalt, 15-20 percent of the waste mineral powder, 25-30 percent of the waste tyre pyrolytic oil, 2-5 percent of petroleum resin, 4-10 percent of a styrene-butadiene-styrene block copolymer and 2-5 percent of styrene-butadiene rubber. The method is simple and easy in process and liable to realize; as for the prepared high-performance modified asphalt product, compared with the traditional conventional modified asphalt material, the softening point greatly raises, the low-temperature performance is good, the viscosity ratio is also lowered compared with rubber asphalt, the high-performance modified asphalt can be widely used for pavements in various grades by replacing other asphalt materials, and a great quantity of solid wastes are used when the using performance of the pavements is remarkably improved, so that petroleum resources are saved, the environment is protected, the cost is also lowered, and the high-performance modified asphalt is beneficial to being widely popularized and applied.
Description
Technical field
The invention belongs to Colophonium preparing technical field is and in particular to a kind of reclaim breeze and damaged tire using asphalt mixing plant
Pyrolysis oil and rubber powder produce high performance modified bitumen method and implement the product that the method is obtained.
Background technology
Building stones used by bituminous concrete produces can produce dust in the production process of rock crushing plant, and dust adhesion is in stone
Asphalt mixing plant can be transported therewith on material.During asphalt mixing stands in bituminous concrete, need building stones are carried out scraper,
Conveying, heating and mix, dust can emit pollution environment, and mixing station needs by bag-type dust collector, dust to be carried out back
Receive.Dust fraction after recovery can be re-added in asphalt, and major part all cannot can only be discarded in use, disposes
Improper meeting land occupation, processing of serious environment pollution, therefore abandoned mine powder is always one of difficult problem perplexing asphalt mixing plant.But
These abandoned mine powder are very little due to volume, and particle diameter, substantially all in below 0.075mm, has good specific surface area, and activity is preferable,
It is easy to react with Colophonium and other materials.These abandoned mine powder have certain intensity simultaneously, are good filleies, permissible
Improve the mechanical property of Colophonium.Most of all, by including SBS and damaged tire with various modified asphalt materials in process of production
There is " grafting " reaction in rubber powder etc., be effectively improved the isolation problem of modified pitch.
And the development with Domestic Automotive Industry, create increasing junked tire.The process of existing junked tire
Mode includes tyre rebuilding, grinds to form rubber powder making reclaimed rubber.Wherein tyre rebuilding has number of times to limit, when renovation is to necessarily
Number of times does not allow for being renovated again, can only discard, and grinds to form rubber powder, and part rubber powder is used for producing road rubber asphalt.Rubber
Glue Colophonium has a good pavement performance, and has the environment protection significance of certain cyclic utilization of waste, is necessarily promoted.But rubber
Asphalt viscosity big it is necessary to produce under the high temperature conditions and building stones mix and stir construction, the flue dust of volatilization is larger, abnormal smells from the patient is heavier, is promoting
During also receive certain resistance.Tire with the addition of substantial amounts of furfural oil in process of production, after furfural oil is reacted with rubber
There is good performance, by junked tire is carried out with Pintsch process, the oily oils and fatss reacted with rubber of original furfural can be analysed
Go out, partly used as inferior fuel, calorific value is not high, but discharge is very serious, therefore domestic limit its use.
Content of the invention
For above-mentioned deficiency, one of the object of the invention is, provides a kind of technique simple, it is easy to accomplish, can be replaced it
Its asphalt material is widely used in each grade road surface, while significantly improving Pavement Condition, in a large number using solid waste
Thing, thus saving petroleum resources, environmental protection, the utilization asphalt mixing plant simultaneously reducing cost reclaims breeze and waste tyre pyrolytic
Oil and rubber powder produce high performance modified bitumen method;
The object of the invention also resides in, and provides a kind of above-mentioned utilization asphalt mixing plant of enforcement to reclaim breeze and waste tyre pyrolytic oil
And rubber powder produces the product that high performance modified bitumen method is obtained.This product can replace other asphalt materials to be widely used in each grade
In road surface, while significantly improving Pavement Condition, in a large number using solid waste, thus saving petroleum resources, protection
Environment, low production cost.
For achieving the above object, technical scheme provided by the present invention is:
One kind reclaims breeze and waste tyre pyrolytic oil using asphalt mixing plant and rubber powder produces high performance modified bitumen method,
It comprises the following steps:
(1) preparing material:Each component of raw material and percentage by weight are as follows:
(2) heating mixing:Junked tire pyrolysis oil is heated to more than 140~160 DEG C, then butadiene-styrene rubber is gradually added
Enter in junked tire pyrolysis oil, be subsequently adding styrene butadiene styrene block copolymer (SBS), and continuous heated and stirred;
(3), when temperature to be heated rises to 170~190 DEG C, sequentially add asphalt, Petropols and abandoned mine powder, wait to stir
After mixing uniformly, make high performance modified bitumen product.
As a modification of the present invention, in described step (2), add styrene-fourth after butadiene-styrene rubber is completely dissolved
Styrene block copolymer.
As a modification of the present invention, described step (3) specifically includes following steps:Temperature to be heated rises to 170~
When 190 DEG C, add asphalt, add Petropols after continuing temperature control stirring 10~40 minutes, then continuously stirred 10~
50 minutes, after being eventually adding the stirring stirring of abandoned mine powder 5~40 minutes, make high performance modified bitumen product.
As a modification of the present invention, described Petropols are C5 Petropols.
As a modification of the present invention, described abandoned mine powder is highway asphalt mixing station in the mistake producing asphalt
The abandoned mine powder reclaiming through bag-type dust in journey, abandoned mine powder particles particle diameter is less than the content of 200 mesh more than 95%, and can only adopt
Heat the recovery breeze that cylinder produces during heating building stones convey mix with gas burner.
As a modification of the present invention, described junked tire pyrolysis oil is that the above truck of diameter 900mm is waste and old
Whole liquids that tire produces through high temperature pyrolysis process.
One kind implements above-mentioned utilization asphalt mixing plant recovery breeze and waste tyre pyrolytic oil and rubber powder production is high-performance modified
The product that Colophonium method is obtained, its each component and percentage by weight are as follows:
Beneficial effects of the present invention are:The technique of the method that the present invention provides is simple, it is easy to accomplish, a certain amount of by adding
The cryogenic property to greatly improve Colophonium for the junked tire pyrolysis oil, reduce its viscosity simultaneously, improve use condition, obtained
Compared with existing routine modified asphalt material, softening point is substantially improved high performance modified bitumen product, low temperature performance well, glues simultaneously
Degree reduces than rubber asphalt, other asphalt materials can be replaced to be widely used in each grade road surface, significantly improving pavement usage
Can while, in a large number using solid waste, thus saving petroleum resources, environmental protection, reduce cost, beneficial to extensively pushing away simultaneously
Wide application.
With reference to embodiment, the invention will be further described.
Specific embodiment
Embodiment 1:One kind that the present embodiment provides utilizes asphalt mixing plant to reclaim breeze and waste tyre pyrolytic oil and rubber powder
Produce high performance modified bitumen method, it comprises the following steps:
(1) preparing material:Each component of raw material and percentage by weight are as follows:Asphalt 40%, abandoned mine powder 15%, waste and old
Tire pyrolysis oil 30%, Petropols 5%, styrene butadiene styrene block copolymer (SBS) (SBS) 5%, butadiene-styrene rubber
5%;
(2) heating mixing:Junked tire pyrolysis oil is heated to more than 140~160 DEG C, then butadiene-styrene rubber is gradually added
Enter in junked tire pyrolysis oil, be subsequently adding styrene butadiene styrene block copolymer (SBS), and continuous heated and stirred;Relatively
Good, add styrene butadiene styrene block copolymer (SBS) after butadiene-styrene rubber is completely dissolved in described step (2).
(3), when temperature to be heated rises to 170~190 DEG C, sequentially add asphalt, Petropols and abandoned mine powder, wait to stir
After mixing uniformly, make high performance modified bitumen product.Preferably, described step (3) specifically includes following steps:Temperature to be heated
When rising to 170~190 DEG C, add asphalt, add Petropols after continuing temperature control stirring 10~40 minutes, then continue
Stirring 10~50 minutes, after being eventually adding the stirring stirring of abandoned mine powder 5~40 minutes, makes high performance modified bitumen product.
Preferably, described Petropols are C5 Petropols.Described abandoned mine powder is that highway asphalt mixing station is producing drip
The abandoned mine powder reclaiming through bag-type dust during blue or green compound, abandoned mine powder particles particle diameter is less than the content of 200 mesh 95%
More than, and the recovery breeze that cylinder produces during heating building stones convey mix can only be heated using gas burner.Described
Whole liquid of producing through high temperature pyrolysis process for diameter 900mm above truck junked tire of junked tire pyrolysis oil
Material.
One kind implements above-mentioned utilization asphalt mixing plant recovery breeze and waste tyre pyrolytic oil and rubber powder production is high-performance modified
The product that Colophonium method is obtained, its each component and percentage by weight are as follows:Asphalt 40%, abandoned mine powder 15%, waste and old wheel
Tire pyrolysis oil 30%, Petropols 5%, styrene butadiene styrene block copolymer (SBS) (SBS) 5%, butadiene-styrene rubber 5%.
Reclaim breeze and waste tyre pyrolytic oil through above-mentioned utilization asphalt mixing plant and rubber powder produces high performance modified bitumen side
Method be obtained high performance modified bitumen product index be:
Project | Unit | Result of the test | Test method |
25 DEG C of needle penetration | 0.1mm | 129 | T0604 |
5 DEG C of ductilities | cm | 73.5 | T0605 |
Softening point (R B) | ℃ | 84.3 | T0606 |
Elastic return | % | 69.2 | T0662 |
Bu Shi rotary viscosity (180 DEG C) | Pa·s | 3.5 | T0611 |
Embodiment 2, one kind that the present embodiment provides utilizes asphalt mixing plant to reclaim breeze and waste tyre pyrolytic oil and rubber powder
Produce high performance modified bitumen method and its product, its component and making step are substantially the same manner as Example 1, and its difference exists
As follows in, each component of raw material and its percentage by weight:Asphalt 50%, abandoned mine powder 15%, junked tire pyrolysis oil 25%,
Petropols 2%, styrene butadiene styrene block copolymer (SBS) (SBS) 4%, butadiene-styrene rubber 4%.
Reclaim breeze and waste tyre pyrolytic oil through above-mentioned utilization asphalt mixing plant and rubber powder produces high performance modified bitumen side
Method be obtained high performance modified bitumen product index be:
Project | Unit | Result of the test | Test method |
25 DEG C of needle penetration | 0.1mm | 99.6 | T0604 |
5 DEG C of ductilities | cm | 44.8 | T0605 |
Softening point (R B) | ℃ | 89.3 | T0606 |
Elastic return | % | 56.2 | T0662 |
Bu Shi rotary viscosity (180 DEG C) | Pa·s | 2.5 | T0611 |
Embodiment 3, one kind that the present embodiment provides utilizes asphalt mixing plant to reclaim breeze and waste tyre pyrolytic oil and rubber powder
Produce high performance modified bitumen method and its product, its component and making step are substantially the same manner as Example 1, and its difference exists
As follows in, each component of raw material and its percentage by weight:Asphalt 45%, abandoned mine powder 16%, junked tire pyrolysis oil 26%,
Petropols 4%, styrene butadiene styrene block copolymer (SBS) (SBS) 7%, butadiene-styrene rubber 2%.
Reclaim breeze and waste tyre pyrolytic oil through above-mentioned utilization asphalt mixing plant and rubber powder produces high performance modified bitumen side
Method be obtained high performance modified bitumen product index be:
Project | Unit | Result of the test | Test method |
25 DEG C of needle penetration | 0.1mm | 89.6 | T0604 |
5 DEG C of ductilities | cm | 75.8 | T0605 |
Softening point (R B) | ℃ | 90.3 | T0606 |
Elastic return | % | 67.6 | T0662 |
Bu Shi rotary viscosity (180 DEG C) | Pa·s | 2.6 | T0611 |
Embodiment 4, one kind that the present embodiment provides utilizes asphalt mixing plant to reclaim breeze and waste tyre pyrolytic oil and rubber powder
Produce high performance modified bitumen method and its product, its component and making step are substantially the same manner as Example 1, and its difference exists
As follows in, each component of raw material and its percentage by weight:Asphalt 40%, abandoned mine powder 15%, junked tire pyrolysis oil 30%,
Petropols 2%, styrene butadiene styrene block copolymer (SBS) (SBS) 10%, butadiene-styrene rubber 3%.
Reclaim breeze and waste tyre pyrolytic oil through above-mentioned utilization asphalt mixing plant and rubber powder produces high performance modified bitumen side
Method be obtained high performance modified bitumen product index be:
Project | Unit | Result of the test | Test method |
25 DEG C of needle penetration | 0.1mm | 110 | T0604 |
5 DEG C of ductilities | cm | 84 | T0605 |
Softening point (R B) | ℃ | 92 | T0606 |
Elastic return | % | 51 | T0662 |
Bu Shi rotary viscosity (180 DEG C) | Pa·s | 2.5 | T0611 |
Embodiment 5, one kind that the present embodiment provides utilizes asphalt mixing plant to reclaim breeze and waste tyre pyrolytic oil and rubber powder
Produce high performance modified bitumen method and its product, its component and making step are substantially the same manner as Example 1, and its difference exists
As follows in, each component of raw material and its percentage by weight:Asphalt 42%, abandoned mine powder 20%, junked tire pyrolysis oil 26%,
Petropols 3%, styrene butadiene styrene block copolymer (SBS) (SBS) 6%, butadiene-styrene rubber 3%.
Must for, the present invention provide method be obtained high performance modified bitumen product with existing routine modified pitch material
Material is compared, and softening point is substantially improved (conventional modified pitch includes Sbs, rubber asphalt, and softening point is typically between 60-70 DEG C),
Cryogenic property greatly improves (conventional modified pitch includes Sbs, rubber asphalt, and ductility is approximately less than 40cm), ratio of viscosities rubber simultaneously
Glue Colophonium reduces.Specifically, the performance parameter of high performance modified bitumen product of the present invention is as follows:
In addition, in other embodiment when carrying out each component ratio selection, can be within the above range according to reality
Need to select, to obtain the product of different specific performance features.
Above-described embodiment is only the preferable embodiment of the present invention, and the present invention can not enumerate out whole embodiment party
Formula, the technical scheme of one of all employing above-described embodiments, or the equivalent variations done according to above-described embodiment, all protect in the present invention
In the range of shield.
The announcement of book and teaching according to the above description, those skilled in the art in the invention can also be to above-mentioned embodiment party
Formula is changed and is changed.Therefore, the invention is not limited in specific embodiment disclosed and described above, to the present invention's
In the scope of the claims that some modifications and changes should also be as fall into the present invention.Although additionally, using in this specification
Some specific terms, but these terms are merely for convenience of description, constitute any restriction to the present invention, using and its
Other Colophonium methods and product obtained from same or similar method and component, all in the scope of the present invention.
Claims (7)
1. one kind reclaims breeze and waste tyre pyrolytic oil using asphalt mixing plant and rubber powder produces high performance modified bitumen method, its
It is characterised by, it comprises the following steps:
(1) preparing material:Each component of raw material and percentage by weight are as follows:
(2) heating mixing:Junked tire pyrolysis oil is heated to more than 140~160 DEG C, then butadiene-styrene rubber is added gradually to
In junked tire pyrolysis oil, it is subsequently adding styrene butadiene styrene block copolymer (SBS), and continuous heated and stirred;
(3), when temperature to be heated rises to 170~190 DEG C, asphalt, Petropols and abandoned mine powder are sequentially added, to be mixed equal
After even, make high performance modified bitumen product.
2. utilization asphalt mixing plant according to claim 1 reclaims breeze and waste tyre pyrolytic oil and rubber powder produces high-performance
Modified pitch method it is characterised in that add after butadiene-styrene rubber is completely dissolved in described step (2) styrene-butadiene-
Styrene block copolymer.
3. utilization asphalt mixing plant according to claim 1 reclaims breeze and waste tyre pyrolytic oil and rubber powder produces high-performance
Modified pitch method is it is characterised in that described step (3) specifically includes following steps:Temperature to be heated rises to 170~190 DEG C
When, add asphalt, add Petropols after continuing temperature control stirring 10~40 minutes, then continuously stirred 10~50 points
Clock, after being eventually adding the stirring stirring of abandoned mine powder 5~40 minutes, makes high performance modified bitumen product.
4. the utilization asphalt mixing plant according to claim 1-3 any one reclaims breeze and waste tyre pyrolytic oil and rubber powder
Produce high performance modified bitumen method it is characterised in that described Petropols are C5 Petropols.
5. the utilization asphalt mixing plant according to claim 1-3 any one reclaims breeze and waste tyre pyrolytic oil and rubber powder
Produce high performance modified bitumen method it is characterised in that described abandoned mine powder is highway asphalt mixing station is producing Colophonium mixing
The abandoned mine powder reclaiming through bag-type dust during material, abandoned mine powder particles particle diameter is less than the content of 200 mesh more than 95%, and
The recovery breeze that cylinder produces during heating building stones convey mix can only be heated using gas burner.
6. the utilization asphalt mixing plant according to claim 1-3 any one reclaims breeze and waste tyre pyrolytic oil and rubber powder
Produce high performance modified bitumen method it is characterised in that described junked tire pyrolysis oil is the above truck of diameter 900mm
Whole liquids that junked tire produces through high temperature pyrolysis process.
7. a kind of described utilization asphalt mixing plant of one of claim 1-6 of implementing reclaims breeze and waste tyre pyrolytic oil and rubber powder life
Produce the prepared product of high performance modified bitumen method it is characterised in that its each component and percentage by weight are as follows: