CN106077476A - A kind of front axle housing body Technology for Heating Processing - Google Patents
A kind of front axle housing body Technology for Heating Processing Download PDFInfo
- Publication number
- CN106077476A CN106077476A CN201610593409.8A CN201610593409A CN106077476A CN 106077476 A CN106077476 A CN 106077476A CN 201610593409 A CN201610593409 A CN 201610593409A CN 106077476 A CN106077476 A CN 106077476A
- Authority
- CN
- China
- Prior art keywords
- dewaxing
- front axle
- hardening
- axle housing
- minute
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Pending
Abstract
The invention discloses a kind of front axle housing body Technology for Heating Processing, 1) dispensing;2) coating;3) hardening;4) dewaxing;5) roasting.Front axle housing body Technology for Heating Processing of the present invention, gained front axle housing rigidity and fatigue resistance performance are effectively improved, and enhance the service life of front axle housing.
Description
Technical field
The present invention relates to a kind of front axle housing body Technology for Heating Processing.
Background technology
The design of casting technique plays a part crux to the quality of casting quality.The front axle housing of wheel excavator is to dig
The security part that pick machine is important.It subjects heavier load and the Moment being continually changing in excavator travels, easily
Curved allusion quotation fatigue fracture phenomenon occur, therefore, front axle housing should have preferable rigidity and fatigue resistance performance.
Summary of the invention
The technical problem to be solved in the present invention is to overcome existing defect, it is provided that a kind of front axle housing body Technology for Heating Processing.
The purpose of the present invention implements by the following technical programs:
A kind of front axle housing body Technology for Heating Processing, including dispensing, coating, hardens, dewaxes and roasting,
Described roasting includes herein below:
Shell mould after dewaxing is put in the box body of only top end opening and is dried 2-4 hour, places wind above the port of box body top
Machine is horizontally dried, and shove charge can carry out high-temperature roasting after drying.
Further:
Described coating includes herein below:
During coating, module repeatedly to move up and down and to rotate, and prevents from collecting between the sand grains of the trough groove on module, aperture or upper strata sand
Trapped air steeps, and removes if any bubble application airduct or hairbrush, and coating local should be avoided to heap simultaneously.
Further:
Described hardening includes herein below:
When hardening with ammonium chloride, before work, the ammonium water in reply hardening pond is stirred, to improve the concentration of ammonium chloride, ammonium chloride
Concentration should be maintained at 21wt%-25wt%;
0.05-0.1% penetrating agent is added, to improve the setting rate of shell mould in hardening pond;
Firm time surface layer is 5-8 minute, and back-up coat is 10-15 minute when there being penetrating agent, does not has during penetrating agent to be that 20-30 divides
Clock;Air-dry time after hardening was advisable with 30-45 minute, should grasp flexibly according to weather simultaneously, winter, capping in rainy season, the summer
Season, dry weather remove the limit.
Further:
Described dewaxing includes herein below:
After formwork hardening painting hangs, dewax after placing 4-8 hour, the floating sand of cup to be blown off before dewaxing;Take off with hot water
During wax, water temperature is 90-98 DEG C, and dewaxing water should avoid boiling phenomenon, dewaxing time to be 20-30 minute, dewaxes in water during dewaxing
Add the technical hydrochloric acid of 1% or the ammonium chloride of 3%-8%, so that shell mould obtains supplementing hardening when dewaxing.
Further:
Described dispensing includes herein below:
First weigh waterglass, refractory powder and activating agent by the weight ratio of 9:4:3, then refractory powder mixed with activating agent,
Again waterglass is poured in the mixture of the two and be stirred simultaneously, mixing time 60-90 minute, then stand 20-30 minute
Can use.
Beneficial effects of the present invention:
Front axle housing body Technology for Heating Processing of the present invention, gained front axle housing rigidity and fatigue resistance performance be effectively improved,
Enhance the service life of front axle housing.
Detailed description of the invention
Hereinafter the preferred embodiments of the present invention are illustrated, it will be appreciated that preferred embodiment described herein is only used
In the description and interpretation present invention, it is not intended to limit the present invention.
A kind of front axle housing body Technology for Heating Processing, including dispensing, coating, hardens, dewaxes and roasting,
Described roasting includes herein below:
Shell mould after dewaxing is put in the box body of only top end opening and is dried 2-4 hour, places wind above the port of box body top
Machine is horizontally dried, and shove charge can carry out high-temperature roasting after drying.
Described coating includes herein below:
During coating, module repeatedly to move up and down and to rotate, and prevents from collecting between the sand grains of the trough groove on module, aperture or upper strata sand
Trapped air steeps, and removes if any bubble application airduct or hairbrush, and coating local should be avoided to heap simultaneously.
Described hardening includes herein below:
When hardening with ammonium chloride, before work, the ammonium water in reply hardening pond is stirred, to improve the concentration of ammonium chloride, ammonium chloride
Concentration should be maintained at 21wt%-25wt%;
0.05-0.1% penetrating agent is added, to improve the setting rate of shell mould in hardening pond;
Firm time surface layer is 5-8 minute, and back-up coat is 10-15 minute when there being penetrating agent, does not has during penetrating agent to be that 20-30 divides
Clock;Air-dry time after hardening was advisable with 30-45 minute, should grasp flexibly according to weather simultaneously, winter, capping in rainy season, the summer
Season, dry weather remove the limit.
Described dewaxing includes herein below:
After formwork hardening painting hangs, dewax after placing 4-8 hour, the floating sand of cup to be blown off before dewaxing;Take off with hot water
During wax, water temperature is 90-98 DEG C, and dewaxing water should avoid boiling phenomenon, dewaxing time to be 20-30 minute, dewaxes in water during dewaxing
Add the technical hydrochloric acid of 1% or the ammonium chloride of 3%-8%, so that shell mould obtains supplementing hardening when dewaxing.
Described dispensing includes herein below:
First weigh waterglass, refractory powder and activating agent by the weight ratio of 9:4:3, then refractory powder mixed with activating agent,
Again waterglass is poured in the mixture of the two and be stirred simultaneously, mixing time 60-90 minute, then stand 20-30 minute
Can use.
The foregoing is only the preferred embodiments of the present invention, be not limited to the present invention, although with reference to aforementioned reality
Executing example to be described in detail the present invention, for a person skilled in the art, it still can be to aforementioned each enforcement
Technical scheme described in example is modified, or wherein portion of techniques feature is carried out equivalent.All essences in the present invention
Within god and principle, any modification, equivalent substitution and improvement etc. made, should be included within the scope of the present invention.
Claims (5)
1. a front axle housing body Technology for Heating Processing, it is characterised in that: include dispensing, coating, harden, dewax and roasting,
Described roasting includes herein below:
Shell mould after dewaxing is put in the box body of only top end opening and is dried 2-4 hour, places wind above the port of box body top
Machine is horizontally dried, and shove charge can carry out high-temperature roasting after drying.
2. a kind of front axle housing body Technology for Heating Processing as claimed in claim 1, it is characterised in that:
Described coating includes herein below:
During coating, module repeatedly to move up and down and to rotate, and prevents from collecting between the sand grains of the trough groove on module, aperture or upper strata sand
Trapped air steeps, and removes if any bubble application airduct or hairbrush, and coating local should be avoided to heap simultaneously.
3. a kind of front axle housing body Technology for Heating Processing as claimed in claim 1, it is characterised in that:
Described hardening includes herein below:
When hardening with ammonium chloride, before work, the ammonium water in reply hardening pond is stirred, to improve the concentration of ammonium chloride, ammonium chloride
Concentration should be maintained at 21wt%-25wt%;
0.05-0.1% penetrating agent is added, to improve the setting rate of shell mould in hardening pond;
Firm time surface layer is 5-8 minute, and back-up coat is 10-15 minute when there being penetrating agent, does not has during penetrating agent to be that 20-30 divides
Clock;Air-dry time after hardening was advisable with 30-45 minute, should grasp flexibly according to weather simultaneously, winter, capping in rainy season, the summer
Season, dry weather remove the limit.
4. a kind of front axle housing body Technology for Heating Processing as claimed in claim 1, it is characterised in that:
Described dewaxing includes herein below:
After formwork hardening painting hangs, dewax after placing 4-8 hour, the floating sand of cup to be blown off before dewaxing;Take off with hot water
During wax, water temperature is 90-98 DEG C, and dewaxing water should avoid boiling phenomenon, dewaxing time to be 20-30 minute, dewaxes in water during dewaxing
Add the technical hydrochloric acid of 1% or the ammonium chloride of 3%-8%, so that shell mould obtains supplementing hardening when dewaxing.
5. a kind of front axle housing body Technology for Heating Processing as claimed in claim 1, it is characterised in that:
Described dispensing includes herein below:
First weigh waterglass, refractory powder and activating agent by the weight ratio of 9:4:3, then refractory powder mixed with activating agent,
Again waterglass is poured in the mixture of the two and be stirred simultaneously, mixing time 60-90 minute, then stand 20-30 minute
Can use.