A kind of papery news media
Technical field
The present invention relates to newsprint technical field, especially relate to a kind of papery news media.
Background technology
Newsprint is the main use paper of newpapers and periodicals and books, needs to meet that papery pine is light, have preferable elasticity, ink absorption
Well, the features such as have certain mechanical strength, opaqueness good.China is paper production, consumption, import big country, with China
The growth of demand for paper products, wood pulp supply much can not meet demand, causes import volume to increase sharply.Wood fibre either from
All it is far above non-wood in performance or technique, but China's forest resourceies are less, China's lumber fibre supply is in decline
Trend.
Waste paper is recycled as Renewable resource, the grass class slurrying of waste paper pulp-making ratio can energy saving in a large number,
Because do not need the maximum cooking section of Sewage water discharge capacity using Deinking Pulp, and the discharge of BOD and COD of deinking wastewater
Amount is easier to be up to state standards after water process.The utilization of secondary stock, solves process paper industry contaminated wastewater and asks
Topic, is also a kind of effective way solving China's wood raw material shortage simultaneously.
China is the country that world's bamboo resource is the abundantest, bamboo class is cultivated and processing and utilization is the longest, cultivated area,
Accumulation and annual production occupy the hat in the world.Bamboo has that easy cultivation, growth be fast, cycle is short, renewable, survival rate is high, the period of felling in turn is short,
The big feature of yield.Bamboo is the raw material being best suitable for papermaking in addition to wood, and the fibre morphology of bamboo wood and content are with needlebush very
Approximately, content of cellulose is high, and fiber is elongated solid, and plasticity is good, and fibre length, between leaf wood and needlebush, is paper pulp
The quality raw materials of papermaking, bamboo paper pulp papermaking has good performance and relatively low cost.
Patent of invention CN1079127C discloses a kind of method that waste paper produces regenerated newsprint, and the method waste paper is
Raw material, adds appropriate NaOH, Na2SiO3In chemical raw material and water, through steaming and decocting, dehydration, bleaching, making beating, purification, copy paper, cut paper
Get product.This invention not only has and can make full use of waste paper regenerated newsprint, thus greatly reducing paper grade (stock) fibril raw material
Consumption and the advantage of consumption of wood, but also there is minimizing environmental pollution, reduce production cost.But secondary stock prepares
Newsprint surface low intensity, bad mechanical property.Patent of invention CN102041747B discloses a kind of environmental protective newsprint paper, is with low
Density polyethylene, linear low density polyethylene, PUR, modified heavy calcium carbonate, modified coal ash preparation obtain.This invention
Paper, with high molecular polymer as substrate material, carries out to Calcium Carbonate and flyash composite modified, and adds other additives, utilizes
The macromolecule interfacial principles of chemistry and macromolecule modified feature, after processing through special process, are combined using polymer mixed, filler
Modified, polymer and filler plasticizing, extrusion curtain coating, calendering formation technique are made, and to energy saving, protect national resource that there have to be non-
Often good meaning.But the newsprint that this invention prepares can not recycle, environment is caused with certain burden.
Content of the invention
In view of this, the purpose of the present invention is for the deficiencies in the prior art, provides a kind of efficent use of resources, protection ring
Border, the papery news media of excellent combination property.
For reaching above-mentioned purpose, the present invention employs the following technical solutions:
A kind of papery news media, including the component of following weight portion:Deinking chemical pulp 60 weight portion, bamboo alkalescence peroxide
Change hydrogen mechanical pulp 18 weight portion, bamboo CTMP 7 weight portion, willow alkaline hydrogen peroxide thermomechanical pulp 15 weight
Part, brightening agent 0.03 ~ 0.08 weight portion, filler 8 ~ 15 weight portion, reinforcing agent 0.5 ~ 1.5 weight portion, retention and drainage aid agent 0.3 ~ 1 weight
Amount part, sizing agent 0.1 ~ 0.3 weight portion.
Preferably, described deinking chemical pulp beating degree is 53 ~ 60 ° of SR, described bamboo APMP making beating
Spend for 45 ~ 50 ° of SR, described bamboo CTMP beating degree is 40 ~ 43 ° of SR, described willow alkaline hydrogen peroxide defibrator process
Mechanical pulp beating degree is 35 ~ 38 ° of SR.
Preferably, described brightening agent is fluorescent whitening agent.
Preferably, described filler is the mixture of neutral winnofil, Magnesiumaluminumsilicate, polyvinyl alcohol and titanium dioxide,
Described neutrality winnofil:Magnesiumaluminumsilicate:Polyvinyl alcohol:The mass ratio of titanium dioxide is 3:1:4:2.
Preferably, described neutrality winnofil is the mixture of prism-shaped crystal and scalenohedron, described prism-shaped
Crystal:The mass ratio of scalenohedron is 2:8~4:6.
Preferably, described reinforcing agent is the mixture of cationic starch, shitosan and methylcellulose, and described cation is formed sediment
Powder:Shitosan:The mass ratio of methylcellulose is 7:1.5:1.5.
Preferably, described retention and drainage aid agent is the mixing of PAMC, polyethylene glycol oxide and polyethyleneimine
Thing, described PAMC:Polyethylene glycol oxide:The mass ratio of polyethyleneimine is 4:3:3.
Preferably, described sizing agent is at least one in alkyl ketene dimer and alkyl succinic anhydride.
Present invention also offers the preparation method of above-mentioned papery news media, by deinking chemical pulp, bamboo alkalescence peroxidating
Hydrogen mechanical pulp, bamboo CTMP and willow alkaline hydrogen peroxide thermomechanical pulp mix homogeneously, in copy paper step
Sequentially add filler, reinforcing agent, brightening agent, sizing agent and retention and drainage aid agent while stirring.
Preferably, when described sizing agent adds, mixed serum pH is 7.0 ~ 7.4.
The invention has the beneficial effects as follows:
1st, the present invention prepares newsprint using secondary stock for primary raw material, solves the present situation of China's timber shortage, meets
Environmental requirement.Excellent long fibre is contained, fibrous binding force is very strong in deinking chemical pulp;Add bamboo alkaline hydrogen peroxide machine
Tool slurry and bamboo CTMP, it is possible to reduce consumption of wood, pulp brightness is high, intensity is high, and yield is high;Add poplar
Tree alkaline hydrogen peroxide thermomechanical pulp can effectively improve pulp strength.
2nd, filler selected by the present invention can improve the optical properties such as whiteness, glossiness and opacity;Improve the flat of paper
Slippery, improves ink absorption, reduces the probability of print through;Improve paper industry structure, improve dimensional stability, and fibre can be replaced
Dimension, reduces production cost.Neutral winnofil adopts the mixture of prism-shaped crystal and scalenohedron, can increase filler
Content and make paper loss of tensile strength minimum.
3rd, reinforcing agent used by the present invention is the mixture of cationic starch, shitosan and methylcellulose, cationic starch
There is good potentiation and retention aid and filtering aid effect, filler can be improved and fiber fines are kept, improve internal bond strength, subtract
Few hair and powder dropping;Shitosan, in addition to there is great amount of hydroxy group, also has the hydroxyl on amino, with methylcellulose, carboxyl etc. and ties
Synthesize hydrogen bond and ionic bond, strengthen the intensity of paper.Reinforcing agent effect used is good, and can reclaim, environmental protection.
4th, efficent use of resources of the present invention, environmental protection;The papery news media preparing, whiteness is high, opacity
Height, intensity is good, excellent combination property.
Specific embodiment
With reference to specific embodiment, the present invention is further elaborated.
A kind of papery news media, including the component of following weight portion:Deinking chemical pulp 60 weight portion, bamboo alkalescence peroxide
Change hydrogen mechanical pulp 18 weight portion, bamboo CTMP 7 weight portion, willow alkaline hydrogen peroxide thermomechanical pulp 15 weight
Part, brightening agent 0.03 ~ 0.08 weight portion, filler 8 ~ 15 weight portion, reinforcing agent 0.5 ~ 1.5 weight portion, retention and drainage aid agent 0.3 ~ 1 weight
Amount part, sizing agent 0.1 ~ 0.3 weight portion.
Described deinking chemical pulp beating degree is preferably 53 ~ 60 ° of SR, and described bamboo APMP beating degree is excellent
Elect 45 ~ 50 ° of SR as, described bamboo CTMP beating degree is preferably 40 ~ 43 ° of SR, described willow alkaline hydrogen peroxide
Thermomechanical pulp beating degree is preferably 35 ~ 38 ° of SR.
Described brightening agent is preferably fluorescent whitening agent, and fluorescent whitening agent can delay newsprint brightness reversion, and factory can be made single
Once bleaching can reach higher whiteness, or reduce bleaching time improve yield and reduce cost.Using fluorescent whitening agent
The whiteness that paper can be made improves without reducing opacity, contains chemical pulp and Deinking Pulp particularly in news paper material,
Fluorescent effect is especially pronounced.
Described filler is preferably neutral winnofil, the mixture of Magnesiumaluminumsilicate, polyvinyl alcohol and titanium dioxide, described
Neutral winnofil:Magnesiumaluminumsilicate:Polyvinyl alcohol:The mass ratio of titanium dioxide is preferably 3:1:4:2, filled can improve
The property of paper, better meets use requirement, saves paper pulp, reduces product cost.Not filled paper, has perhaps between fiber
How tiny space, paper is coarse uneven, affects printing quality, lead to that trace is deep mixed, smudgy, handling property relatively
Difference.Plus with after filler, filler is scattered between fiber, and hole is filled and led up, and can improve flexibility and the plasticity of paper.Neutral
Winnofil can preferably improve the opacity of paper, increase the oil absorbency of paper, and its brightness is larger, becomes paper soft
Soft, tight and glossy, the physical strength of paper is affected less;The whiteness of Magnesiumaluminumsilicate, weatherability and oil factor are all higher, than
Surface area is big, wearing valve and bulk density are relatively low, and Magnesiumaluminumsilicate is filled with the whiteness of newsprint and opacity is higher, tensile strength
Close with color density, print through value is relatively low;Compounded using Magnesiumaluminumsilicate/neutrality winnofil and be filled with, filler can be significantly improved
Retention, improve newsprint optical property, simultaneously also can effective control production cost;Light basis weight of manufacturing paper with pulp is filled with using Magnesiumaluminumsilicate
Newsprint, can significantly improve into paper optical property and printing performance, reduce paper print through, and Magnesiumaluminumsilicate has reduction newsprint
Quantitative potentiality.
Described neutrality winnofil is preferably the mixture of prism-shaped crystal and scalenohedron, and described prism-shaped is brilliant
Body:The mass ratio of scalenohedron is preferably 2:8~4:6, neutral winnofil has three kinds of forms:Scalenohedron, tiltedly square
Hexahedral, prism-shaped.Prism crystal is single solid, shaped granule in substrate, and it can make paper hole few, opacity
High;Tiltedly the hexahedro crystal in side plays similar effect, but effect is smaller, also slightly difference in form;The knot that scalenohedron opens wide
Structure makes paper porous and provides bulk and whiteness.Prism-shaped crystal neutrality winnofil and scalenohedron are neutral heavy
Shallow lake Calcium Carbonate is used in mixed way, and can increase the content of filler and make the loss of tensile strength minimum of paper.
Described reinforcing agent is preferably the mixture of cationic starch, shitosan and methylcellulose, described cationic starch:
Shitosan:The mass ratio of methylcellulose is preferably 7:1.5:1.5.The preparation method of described reinforcing agent is:(1)In 7 weight portions
Add the water of 25 ~ 30 weight portions in cationic starch, 1.5 weight portion shitosans and 1.5 weight portion methylcellulose mixture, stir
Mix uniformly;(2)In step(1)Cationic starch, shitosan and methylcellulose gross weight 0.1% is added in the mixture obtaining
Amylase and 0.01% cellulase, pH is adjusted to 5.0 ~ 6.5, digests 5 ~ 10min, wherein diastatic enzyme activity is 5 ×
104U/g, the enzyme activity of cellulase is 80 × 104U/g;(3)By step(2)The enzymatic hydrolysate obtaining is heated to 80 ~ 95 DEG C, protects
Warm 5 ~ 8min, then cooling, dry, pulverizing, obtain described reinforcing agent.Reinforcing agent can with augmentor fiber between Hydrogen bonding forces,
To improve paper physical intensity, cationic starch has good enhancing retention aid and filtering aid effect, can improve filler and tiny fibre
Dimension is kept, and improves internal bond strength, reduces hair and powder dropping;Shitosan, in addition to there is great amount of hydroxy group, also has amino, with methyl
Hydroxyl on cellulose, carboxyl etc. are combined into hydrogen bond and ionic bond, strengthen the intensity of paper.
Described retention and drainage aid agent is preferably the mixture of PAMC, polyethylene glycol oxide and polyethyleneimine,
Described PAMC:Polyethylene glycol oxide:The mass ratio of polyethyleneimine is preferably 4:3:3, cation polypropylene acyl
Amine and polyethyleneimine compounding use, can be greatly improved clear water effect;Polyethylene glycol oxide is except playing the role of bridging and bonding
Outside moreover it is possible to suspension solid contents some in slurry formed uniqueness network and have retention effect.
Described sizing agent is preferably at least one in alkyl ketene dimer and alkyl succinic anhydride, and applying glue can make paper
Or cardboard has the performance resisting liquid diffusion and infiltration, to improve surface strength, reduce and eliminate the hair loss in printing process
Dry linting phenomenon.
Present invention also offers the preparation method of above-mentioned papery news media, by deinking chemical pulp, bamboo alkalescence peroxidating
Hydrogen mechanical pulp, bamboo CTMP and willow alkaline hydrogen peroxide thermomechanical pulp mix homogeneously, in copy paper step
Sequentially add filler, reinforcing agent, brightening agent, sizing agent and retention and drainage aid agent while stirring.Mixing slurry when described sizing agent adds
Liquid pH is preferably 7.0 ~ 7.4, and in the range of this, sizing efficiency reaches optimum level.
Below by specific embodiment, so that those skilled in the art can be implemented.
Embodiment 1
A kind of papery news media, including the component of following weight portion:Beating degree is deinking chemical pulp 60 weight of 53 ° of SR
Part, beating degree is bamboo APMP 18 weight portion of 45 ° of SR, and beating degree is the bamboo chemistry defibrator process of 40 ° of SR
Mechanical pulp 7 weight portion, beating degree is willow alkaline hydrogen peroxide thermomechanical pulp 15 weight portion of 35 ° of SR, brightening agent 0.03 weight
Amount part, filler 8 weight portion, reinforcing agent 0.5 weight portion, retention and drainage aid agent 0.3 weight portion, sizing agent 0.1 weight portion.
Wherein, filler is the mixture of neutral winnofil, Magnesiumaluminumsilicate, polyvinyl alcohol and titanium dioxide, neutral heavy
Shallow lake Calcium Carbonate:Magnesiumaluminumsilicate:Polyvinyl alcohol:The mass ratio of titanium dioxide is 3:1:4:2.Neutral winnofil is that prism-shaped is brilliant
Body and the mixture of scalenohedron, prism-shaped crystal:The mass ratio of scalenohedron is 2:8.
Reinforcing agent is the mixture of cationic starch, shitosan and methylcellulose(Cationic starch:Shitosan:Methyl
The mass ratio of cellulose is preferably 7:1.5:1.5), the preparation method of reinforcing agent is:(1)7 weight portion cationic starches, 1.5
Add the water of 28 weight portions in weight portion shitosan and 1.5 weight portion methylcellulose mixture, stir;(2)In step
(1)Cationic starch, the amylase of shitosan and methylcellulose gross weight 0.1% and 0.01% is added in the mixture obtaining
Cellulase, pH is adjusted to 6.0, digests 8min, and wherein diastatic enzyme activity is 5 × 104U/g, the enzyme activity of cellulase
For 80 × 104U/g;(3)By step(2)The enzymatic hydrolysate obtaining is heated to 90 DEG C, is incubated 6min, then cooling, dry, powder
Broken, obtain reinforcing agent.
Brightening agent is fluorescent whitening agent.
Retention and drainage aid agent is the mixture of PAMC, polyethylene glycol oxide and polyethyleneimine, and cation is gathered
Acrylamide:Polyethylene glycol oxide:The mass ratio of polyethyleneimine is 4:3:3.
Sizing agent is alkyl ketene dimer.
The preparation method of above-mentioned papery news media, by deinking chemical pulp, bamboo APMP, bamboo
Learn thermomechanical pulp and willow alkaline hydrogen peroxide thermomechanical pulp mix homogeneously, sequentially add while stirring in copy paper step
Filler, reinforcing agent, brightening agent, sizing agent and retention and drainage aid agent.When sizing agent adds, mixed serum pH is 7.0.
Embodiment 2
A kind of papery news media, including the component of following weight portion:Beating degree is deinking chemical pulp 60 weight of 54 ° of SR
Part, beating degree is bamboo APMP 18 weight portion of 46 ° of SR, and beating degree is the bamboo chemistry defibrator process of 41 ° of SR
Mechanical pulp 7 weight portion, beating degree is willow alkaline hydrogen peroxide thermomechanical pulp 15 weight portion of 36 ° of SR, brightening agent 0.04 weight
Amount part, filler 9 weight portion, reinforcing agent 0.6 weight portion, retention and drainage aid agent 0.4 weight portion, sizing agent 0.15 weight portion.
Wherein, filler is the mixture of neutral winnofil, Magnesiumaluminumsilicate, polyvinyl alcohol and titanium dioxide, neutral heavy
Shallow lake Calcium Carbonate:Magnesiumaluminumsilicate:Polyvinyl alcohol:The mass ratio of titanium dioxide is 3:1:4:2.Neutral winnofil is that prism-shaped is brilliant
Body and the mixture of scalenohedron, prism-shaped crystal:The mass ratio of scalenohedron is 3:7.
Reinforcing agent is the mixture of cationic starch, shitosan and methylcellulose(Cationic starch:Shitosan:Methyl
The mass ratio of cellulose is preferably 7:1.5:1.5), brightening agent is fluorescent whitening agent.
Retention and drainage aid agent is the mixture of PAMC, polyethylene glycol oxide and polyethyleneimine, and cation is gathered
Acrylamide:Polyethylene glycol oxide:The mass ratio of polyethyleneimine is 4:3:3.
Sizing agent is alkyl ketene dimer.
The preparation method of above-mentioned papery news media, by deinking chemical pulp, bamboo APMP, bamboo
Learn thermomechanical pulp and willow alkaline hydrogen peroxide thermomechanical pulp mix homogeneously, sequentially add while stirring in copy paper step
Filler, reinforcing agent, brightening agent, sizing agent and retention and drainage aid agent.When sizing agent adds, mixed serum pH is 7.1.
Embodiment 3
A kind of papery news media, including the component of following weight portion:Beating degree is deinking chemical pulp 60 weight of 55 ° of SR
Part, beating degree is bamboo APMP 18 weight portion of 47 ° of SR, and beating degree is the bamboo chemistry defibrator process of 42 ° of SR
Mechanical pulp 7 weight portion, beating degree is willow alkaline hydrogen peroxide thermomechanical pulp 15 weight portion of 37 ° of SR, brightening agent 0.05 weight
Amount part, filler 10 weight portion, reinforcing agent 0.7 weight portion, retention and drainage aid agent 0.5 weight portion, sizing agent 0.2 weight portion.
Wherein, filler is the mixture of neutral winnofil, Magnesiumaluminumsilicate, polyvinyl alcohol and titanium dioxide, neutral heavy
Shallow lake Calcium Carbonate:Magnesiumaluminumsilicate:Polyvinyl alcohol:The mass ratio of titanium dioxide is 3:1:4:2.Neutral winnofil is that prism-shaped is brilliant
Body and the mixture of scalenohedron, prism-shaped crystal:The mass ratio of scalenohedron is 4:6.
Reinforcing agent is the mixture of cationic starch, shitosan and methylcellulose(Cationic starch:Shitosan:Methyl
The mass ratio of cellulose is preferably 7:1.5:1.5), brightening agent is fluorescent whitening agent.
Retention and drainage aid agent is the mixture of PAMC, polyethylene glycol oxide and polyethyleneimine, and cation is gathered
Acrylamide:Polyethylene glycol oxide:The mass ratio of polyethyleneimine is 4:3:3.
Sizing agent is alkyl succinic anhydride.
The preparation method of above-mentioned papery news media, by deinking chemical pulp, bamboo APMP, bamboo
Learn thermomechanical pulp and willow alkaline hydrogen peroxide thermomechanical pulp mix homogeneously, sequentially add while stirring in copy paper step
Filler, reinforcing agent, brightening agent, sizing agent and retention and drainage aid agent.When sizing agent adds, mixed serum pH is 7.2.
Embodiment 4
A kind of papery news media, including the component of following weight portion:Beating degree is deinking chemical pulp 60 weight of 56 ° of SR
Part, beating degree is bamboo APMP 18 weight portion of 48 ° of SR, and beating degree is the bamboo chemistry defibrator process of 43 ° of SR
Mechanical pulp 7 weight portion, beating degree is willow alkaline hydrogen peroxide thermomechanical pulp 15 weight portion of 37 ° of SR, brightening agent 0.06 weight
Amount part, filler 11 weight portion, reinforcing agent 0.8 weight portion, retention and drainage aid agent 0.6 weight portion, sizing agent 0.25 weight portion.
Wherein, filler is the mixture of neutral winnofil, Magnesiumaluminumsilicate, polyvinyl alcohol and titanium dioxide, neutral heavy
Shallow lake Calcium Carbonate:Magnesiumaluminumsilicate:Polyvinyl alcohol:The mass ratio of titanium dioxide is 3:1:4:2.Neutral winnofil is that prism-shaped is brilliant
Body and the mixture of scalenohedron, prism-shaped crystal:The mass ratio of scalenohedron is 2.5:7.5.
Reinforcing agent is the mixture of cationic starch, shitosan and methylcellulose(Cationic starch:Shitosan:Methyl
The mass ratio of cellulose is preferably 7:1.5:1.5), brightening agent is fluorescent whitening agent.
Retention and drainage aid agent is the mixture of PAMC, polyethylene glycol oxide and polyethyleneimine, and cation is gathered
Acrylamide:Polyethylene glycol oxide:The mass ratio of polyethyleneimine is 4:3:3.
Sizing agent is alkyl succinic anhydride.
The preparation method of above-mentioned papery news media, by deinking chemical pulp, bamboo APMP, bamboo
Learn thermomechanical pulp and willow alkaline hydrogen peroxide thermomechanical pulp mix homogeneously, sequentially add while stirring in copy paper step
Filler, reinforcing agent, brightening agent, sizing agent and retention and drainage aid agent.When sizing agent adds, mixed serum pH is 7.3.
Embodiment 5
A kind of papery news media, including the component of following weight portion:Beating degree is deinking chemical pulp 60 weight of 57 ° of SR
Part, beating degree is bamboo APMP 18 weight portion of 49 ° of SR, and beating degree is the bamboo chemistry defibrator process of 40 ° of SR
Mechanical pulp 7 weight portion, beating degree is willow alkaline hydrogen peroxide thermomechanical pulp 15 weight portion of 38 ° of SR, brightening agent 0.07 weight
Amount part, filler 12 weight portion, reinforcing agent 0.9 weight portion, retention and drainage aid agent 0.7 weight portion, sizing agent 0.3 weight portion.
Wherein, filler is the mixture of neutral winnofil, Magnesiumaluminumsilicate, polyvinyl alcohol and titanium dioxide, neutral heavy
Shallow lake Calcium Carbonate:Magnesiumaluminumsilicate:Polyvinyl alcohol:The mass ratio of titanium dioxide is 3:1:4:2.Neutral winnofil is that prism-shaped is brilliant
Body and the mixture of scalenohedron, prism-shaped crystal:The mass ratio of scalenohedron is 3.5:6.5.
Reinforcing agent is the mixture of cationic starch, shitosan and methylcellulose(Cationic starch:Shitosan:Methyl
The mass ratio of cellulose is preferably 7:1.5:1.5), brightening agent is fluorescent whitening agent.
Retention and drainage aid agent is the mixture of PAMC, polyethylene glycol oxide and polyethyleneimine, and cation is gathered
Acrylamide:Polyethylene glycol oxide:The mass ratio of polyethyleneimine is 4:3:3.
Sizing agent is the mixture of alkyl ketene dimer and alkyl succinic anhydride, mixed proportion be arbitrarily than.
The preparation method of above-mentioned papery news media, by deinking chemical pulp, bamboo APMP, bamboo
Learn thermomechanical pulp and willow alkaline hydrogen peroxide thermomechanical pulp mix homogeneously, sequentially add while stirring in copy paper step
Filler, reinforcing agent, brightening agent, sizing agent and retention and drainage aid agent.When sizing agent adds, mixed serum pH is 7.4.
Embodiment 6
A kind of papery news media, including the component of following weight portion:Beating degree is deinking chemical pulp 60 weight of 58 ° of SR
Part, beating degree is bamboo APMP 18 weight portion of 50 ° of SR, and beating degree is the bamboo chemistry defibrator process of 41 ° of SR
Mechanical pulp 7 weight portion, beating degree is willow alkaline hydrogen peroxide thermomechanical pulp 15 weight portion of 35 ° of SR, brightening agent 0.08 weight
Amount part, filler 13 weight portion, reinforcing agent 1.1 weight portion, retention and drainage aid agent 0.8 weight portion, sizing agent 0.15 weight portion.
Wherein, filler is the mixture of neutral winnofil, Magnesiumaluminumsilicate, polyvinyl alcohol and titanium dioxide, neutral heavy
Shallow lake Calcium Carbonate:Magnesiumaluminumsilicate:Polyvinyl alcohol:The mass ratio of titanium dioxide is 3:1:4:2.Neutral winnofil is that prism-shaped is brilliant
Body and the mixture of scalenohedron, prism-shaped crystal:The mass ratio of scalenohedron is 2:8.
Reinforcing agent is the mixture of cationic starch, shitosan and methylcellulose(Cationic starch:Shitosan:Methyl
The mass ratio of cellulose is preferably 7:1.5:1.5), brightening agent is fluorescent whitening agent.
Retention and drainage aid agent is the mixture of PAMC, polyethylene glycol oxide and polyethyleneimine, and cation is gathered
Acrylamide:Polyethylene glycol oxide:The mass ratio of polyethyleneimine is 4:3:3.
Sizing agent be alkyl ketene dimer and alkyl succinic anhydride mixture, mixed proportion be arbitrarily than.
The preparation method of above-mentioned papery news media, by deinking chemical pulp, bamboo APMP, bamboo
Learn thermomechanical pulp and willow alkaline hydrogen peroxide thermomechanical pulp mix homogeneously, sequentially add while stirring in copy paper step
Filler, reinforcing agent, brightening agent, sizing agent and retention and drainage aid agent.When sizing agent adds, mixed serum pH is 7.2.
Embodiment 7
A kind of papery news media, including the component of following weight portion:Beating degree is deinking chemical pulp 60 weight of 59 ° of SR
Part, beating degree is bamboo APMP 18 weight portion of 46 ° of SR, and beating degree is the bamboo chemistry defibrator process of 42 ° of SR
Mechanical pulp 7 weight portion, beating degree is willow alkaline hydrogen peroxide thermomechanical pulp 15 weight portion of 37 ° of SR, brightening agent 0.06 weight
Amount part, filler 14 weight portion, reinforcing agent 1.4 weight portion, retention and drainage aid agent 0.9 weight portion, sizing agent 0.25 weight portion.
Wherein, filler is the mixture of neutral winnofil, Magnesiumaluminumsilicate, polyvinyl alcohol and titanium dioxide, neutral heavy
Shallow lake Calcium Carbonate:Magnesiumaluminumsilicate:Polyvinyl alcohol:The mass ratio of titanium dioxide is 3:1:4:2.Neutral winnofil is that prism-shaped is brilliant
Body and the mixture of scalenohedron, prism-shaped crystal:The mass ratio of scalenohedron is 3:7.
Reinforcing agent is the mixture of cationic starch, shitosan and methylcellulose(Cationic starch:Shitosan:Methyl
The mass ratio of cellulose is preferably 7:1.5:1.5), brightening agent is fluorescent whitening agent.
Retention and drainage aid agent is the mixture of PAMC, polyethylene glycol oxide and polyethyleneimine, and cation is gathered
Acrylamide:Polyethylene glycol oxide:The mass ratio of polyethyleneimine is 4:3:3.
Sizing agent is alkyl ketene dimer.
The preparation method of above-mentioned papery news media, by deinking chemical pulp, bamboo APMP, bamboo
Learn thermomechanical pulp and willow alkaline hydrogen peroxide thermomechanical pulp mix homogeneously, sequentially add while stirring in copy paper step
Filler, reinforcing agent, brightening agent, sizing agent and retention and drainage aid agent.When sizing agent adds, mixed serum pH is 7.3.
Embodiment 8
A kind of papery news media, including the component of following weight portion:Beating degree is deinking chemical pulp 60 weight of 60 ° of SR
Part, beating degree is bamboo APMP 18 weight portion of 50 ° of SR, and beating degree is the bamboo chemistry defibrator process of 43 ° of SR
Mechanical pulp 7 weight portion, beating degree is willow alkaline hydrogen peroxide thermomechanical pulp 15 weight portion of 38 ° of SR, brightening agent 0.08 weight
Amount part, filler 15 weight portion, reinforcing agent 1.5 weight portion, retention and drainage aid agent 1 weight portion, sizing agent 0.3 weight portion.
Wherein, filler is the mixture of neutral winnofil, Magnesiumaluminumsilicate, polyvinyl alcohol and titanium dioxide, neutral heavy
Shallow lake Calcium Carbonate:Magnesiumaluminumsilicate:Polyvinyl alcohol:The mass ratio of titanium dioxide is 3:1:4:2.Neutral winnofil is that prism-shaped is brilliant
Body and the mixture of scalenohedron, prism-shaped crystal:The mass ratio of scalenohedron is 4:6.
Reinforcing agent is the mixture of cationic starch, shitosan and methylcellulose(Cationic starch:Shitosan:Methyl
The mass ratio of cellulose is preferably 7:1.5:1.5), brightening agent is fluorescent whitening agent.
Retention and drainage aid agent is the mixture of PAMC, polyethylene glycol oxide and polyethyleneimine, and cation is gathered
Acrylamide:Polyethylene glycol oxide:The mass ratio of polyethyleneimine is 4:3:3.
Sizing agent is alkyl succinic anhydride.
The preparation method of above-mentioned papery news media, by deinking chemical pulp, bamboo APMP, bamboo
Learn thermomechanical pulp and willow alkaline hydrogen peroxide thermomechanical pulp mix homogeneously, sequentially add while stirring in copy paper step
Filler, reinforcing agent, brightening agent, sizing agent and retention and drainage aid agent.When sizing agent adds, mixed serum pH is 7.4.
Finally illustrate, only in order to technical scheme to be described and unrestricted, this area is common for above example
Other modifications or equivalent that technical staff is made to technical scheme, without departing from technical solution of the present invention
Spirit and scope, all should cover in the middle of scope of the presently claimed invention.