CN105170339B - The method for floating of sulphur oxygen mixed mineral in a kind of recovery mine tailing - Google Patents

The method for floating of sulphur oxygen mixed mineral in a kind of recovery mine tailing Download PDF

Info

Publication number
CN105170339B
CN105170339B CN201510639371.9A CN201510639371A CN105170339B CN 105170339 B CN105170339 B CN 105170339B CN 201510639371 A CN201510639371 A CN 201510639371A CN 105170339 B CN105170339 B CN 105170339B
Authority
CN
China
Prior art keywords
mineral
ore
makees
mine tailing
sulphur oxygen
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Active
Application number
CN201510639371.9A
Other languages
Chinese (zh)
Other versions
CN105170339A (en
Inventor
魏宗武
穆枭
石倡溶
梁绍华
蒋文俊
周善鹏
管继炜
王娜
刘萌
邓建
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Guangdong Gaohang Intellectual Property Operation Co ltd
QIDONG COUNTY NIAOJIANG DALING LEAD AND ZINC MINING INDUSTRY Co.,Ltd.
Original Assignee
Guangxi University
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Guangxi University filed Critical Guangxi University
Priority to CN201510639371.9A priority Critical patent/CN105170339B/en
Publication of CN105170339A publication Critical patent/CN105170339A/en
Application granted granted Critical
Publication of CN105170339B publication Critical patent/CN105170339B/en
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

The method for floating of sulphur oxygen mixed mineral in a kind of recovery mine tailing, pH regulators are made using sulfuric acid, calgon makees mineral dispersant, vulcanized sodium, ammonium sulfate, copper sulphate make the activator of composite ore, mercaptan makees composite ore collecting agent with butyl xanthate, and 2# oil makees foaming agent and obtains bulk concentrate to the progress flotation of sulphur oxygen composite ore.Sulphur oxygen composite ore in mine tailing can effectively be reclaimed using the present invention, it is being that 0.28%~1.07%, antimony grade is under the conditions of 0.24%~0.83% to ore deposit lead grade, it is the lead antimony compound refined mine that 20.87%~34.55%, antimony grade is 17.53%~28.40% to result in lead grade by the inventive method, and lead recovery is that 75.21%~82.77%, antimony recovery is 73.60%~80.75%.

Description

The method for floating of sulphur oxygen mixed mineral in a kind of recovery mine tailing
First, technical field
It is particularly a kind of to reclaim sulphur oxygen composite ore in mine tailing the present invention relates to a kind of flotation recovery method of sulphur oxygen composite ore The method for floating of thing.
2nd, background technology
In multi-metal sulfide ore dressing, some metalliferous minerals are because disseminated grain size is thin, surface oxidation, liberation degree of minerals not The reasons such as enough, technical merit and lose in mine tailing.These mine tailings are because useful value is low, bond agglomerating, surface oxidation, embedding cloth Fine size and it is mixed with debris and is stored in by long-term heap in Tailings Dam;As the time stored up is longer, the valuable mineral surface in mine tailing Aoxidize deeper, the difficulty of valuable metal recovery is bigger.As mineral resources are petered out, metal price is gone up, Tailings Dam The metalliferous mineral of middle-low grade then turns into valuable secondary resource, how to reclaim as far as possible the secondary resource of this partial surface oxidation into The focus studied for current ore dressing circle.
3rd, the content of the invention
It is an object of the invention to provide a kind of method for floating for reclaiming sulphur oxygen mixed mineral in mine tailing, it can reclaim tail The metalliferous mineral of valuable sulphide ore and sulphide ore surface oxidation in ore deposit.
The present invention reaches above-mentioned purpose using following technical scheme:The flotation side of sulphur oxygen mixed mineral in a kind of recovery mine tailing Method, specific steps and regime of agent are as follows:
(1) pH regulators are made with sulfuric acid,
(2) mineral dispersant is made with calgon,
(3) vulcanized sodium, ammonium sulfate, copper sulphate make composite ore activator,
(4) mercaptan makees composite ore collecting agent with butyl xanthate,
(5) 2# oil makees foaming agent,
(6) in floatation process, after mine tailing ore grinding to mineral monomer dissociation, add sulfuric acid and adjust pH5.5~6, by six inclined phosphorus Sour sodium makees mineral dispersant, and vulcanized sodium, ammonium sulfate, copper sulphate make composite ore activator, and mercaptan is caught with butyl xanthate as composite ore Agent is received, 2# oil makees foaming agent and carries out collecting to composite ore, and scanning recleaning three times by one roughing obtains bulk concentrate,
(7) the total consumption of medicament is:
The described method for floating for reclaiming sulphur oxygen mixed mineral in mine tailing, in use, the medicament is first configured to following Concentration expressed in percentage by weight:
Unless otherwise indicated, percentage of the present invention is mass percent, and each component content percentage sum is 100%.
The present invention's has the prominent advantages that:
1st, the sulphur oxygen composite ore in mine tailing can simultaneously be reclaimed, obtains more high-grade bulk concentrate and high recovery Rate.
2nd, can be to resource comprehensive utilization, and flow is simple.
4th, embodiment
Embodiment 1
An application example of the method for floating of sulphur oxygen mixed mineral in recovery mine tailing of the present invention, including following step Suddenly:
1. raw mineral materials:
Raw mineral materials used is lead antimony zinc sulphur oxygen composite ore, and lead content is 0.28%, antimony 0.24%, zinc in ore 1.26%th, sulphur 5.63%.Material phase analysis shows:Lead antimony mineral is based on jamesonite, separately containing a small amount of galena, stibnite, Zinc mineral is so that containing based on marmatite, separately containing a small amount of zincblende, sulfur mineral is based on pyrite, magnetic iron ore, separately containing a small amount of arsenic Pyrite.Lead oxidation rate is up to 24.27% in ore, and antimony oxygenation efficiency is up to 28.10%, and zinc oxygenation efficiency is up to 19.65%.
2. floating agent and operating condition:
In floatation process, after ore ore grinding to mineral monomer dissociation, add sodium carbonate and adjust pH7.5~8, by hexa metaphosphoric acid Sodium makees fine mud mineral dispersant, and zinc sulfate makees other mineral inhibitors, vulcanized sodium, ammonium hydrogen carbonate, plumbi nitras with calcium hypochlorite Make lead antimony mineral activator, diethyldithiocarbamate makees lead antimony mineral collecting agent with butyl xanthate, and 2# oil makees foaming agent to sulphur oxygen lead antimony mineral Carry out collecting.Result of the test shows, effectively can be reclaimed sulphur oxygen mixed lead antimony ore using process above and agentia condition, It is being 0.28%, under conditions of antimony content 0.24% to ore deposit lead content, it is selected twice by three times three choosings of one roughing, finally obtain It is 20.87%, antimony grade 17.53% to obtain lead grade, and the rate of recovery is respectively 75.21% and 73.60% mixing lead-antimony concentrate.
Embodiment 2
Another application example of the method for floating of sulphur oxygen mixed mineral in recovery mine tailing of the present invention, including it is as follows Step:
1. raw mineral materials:
Raw mineral materials used is lead antimony zinc sulphur oxygen composite ore, and lead content is 1.07%, antimony 0.83%, zinc in ore 3.20%th, sulphur 7.36%.Material phase analysis shows:Lead minerals is based on galena, and separately containing a small amount of cerussite, antimony is based on brightness antimony Ore deposit, zinc mineral is with containing based on zincblende, separately containing a small amount of marmatite, and sulfur mineral is another containing a small amount of based on pyrite, mispickel Magnetic iron ore.Lead oxidation rate is up to 30.50% in ore, and antimony oxygenation efficiency is up to 33.52%, and zinc oxygenation efficiency is up to 21.70%.
2. floating agent and operating condition:
In floatation process, after ore ore grinding to mineral monomer dissociation, add sodium carbonate and adjust pH7.5~8, by hexa metaphosphoric acid Sodium makees fine mud mineral dispersant, and zinc sulfate makees other mineral inhibitors, vulcanized sodium, ammonium hydrogen carbonate, plumbi nitras with calcium hypochlorite Make lead antimony mineral activator, diethyldithiocarbamate makees lead antimony mineral collecting agent with butyl xanthate, and 2# oil makees foaming agent to sulphur oxygen lead antimony mineral Carry out collecting.Result of the test shows, effectively can be reclaimed sulphur oxygen mixed lead antimony ore using process above and agentia condition, It is being 1.07%, under conditions of antimony content 0.83% to ore deposit lead content, it is selected twice by three times three choosings of one roughing, finally obtain It is 34.55%, the mixing lead-antimony concentrate of antimony grade 28.40% to obtain lead grade, and lead recovery is 82.77%, and antimony recovery is 80.75%.

Claims (2)

1. a kind of method for floating for reclaiming sulphur oxygen mixed mineral in mine tailing, it is characterised in that specific steps and regime of agent are as follows:
(1) pH regulators are made with sulfuric acid,
(2) mineral dispersant is made with calgon,
(3) vulcanized sodium, ammonium sulfate, copper sulphate make composite ore activator,
(4) mercaptan makees composite ore collecting agent with butyl xanthate,
(5) 2# oil makees foaming agent,
(6) in floatation process, after mine tailing ore grinding to mineral monomer dissociation, add sulfuric acid and adjust pH5.5~6, by calgon Make mineral dispersant, vulcanized sodium, ammonium sulfate, copper sulphate make composite ore activator, and mercaptan makees composite ore collecting agent with butyl xanthate, 2# oil makees foaming agent and carries out collecting to composite ore, and scanning recleaning three times by one roughing obtains bulk concentrate,
(7) the total consumption of medicament is:
2. the method for floating according to claim 1 for reclaiming sulphur oxygen mixed mineral in mine tailing, it is characterised in that in use, The medicament is first configured to following concentration expressed in percentage by weight:
CN201510639371.9A 2015-09-30 2015-09-30 The method for floating of sulphur oxygen mixed mineral in a kind of recovery mine tailing Active CN105170339B (en)