CN1048234A - Goose down fur and ripening process thereof - Google Patents

Goose down fur and ripening process thereof Download PDF

Info

Publication number
CN1048234A
CN1048234A CN 89105111 CN89105111A CN1048234A CN 1048234 A CN1048234 A CN 1048234A CN 89105111 CN89105111 CN 89105111 CN 89105111 A CN89105111 A CN 89105111A CN 1048234 A CN1048234 A CN 1048234A
Authority
CN
China
Prior art keywords
dermatotome
hour
goose
shortening
fur
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CN 89105111
Other languages
Chinese (zh)
Inventor
杜方甫
张昆勤
刘聚芳
李连印
高桂敏
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
fur CAP FACTORY OF FUSHUN CITY
Original Assignee
fur CAP FACTORY OF FUSHUN CITY
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by fur CAP FACTORY OF FUSHUN CITY filed Critical fur CAP FACTORY OF FUSHUN CITY
Priority to CN 89105111 priority Critical patent/CN1048234A/en
Publication of CN1048234A publication Critical patent/CN1048234A/en
Pending legal-status Critical Current

Abstract

The present invention relates to a kind of goose down fur product and ripening process thereof, belong to leather shortening technical field.Goose down fur is that goose is slaughtered the back peeling, dials and goes big hair after the fur that shortening forms.Its ripening process has adopted group hair, degreasing, has soaked nitre, has pasted steps such as shovel, shortening, oven dry, stuffing, perching.Goose down fur product through shortening processing has abundant fine hair, and thermal property is good, and fine hair is pure white, the dermatotome softness, and outward appearance is good, and its tensile strength and pliability can compare favourably with animal skin.

Description

Goose down fur and ripening process thereof
The present invention relates to a kind of goose down fur product and ripening process thereof, belong to leather shortening technical field.
In technique known, the shortening of fur refers to the shortening of beasts fur more, the various animal skin hairs behind the shortening, and thermal property is good, has been widely used in industries such as clothes, and is very popular.Yet, the strong animal of cold hardiness in winter is also arranged, in the bird as goose.It has numerous thick feather and plentiful fine hair, but in the past in people's the winter protection article, has only utilized the fine hair of goose, and goose fur at home and abroad utilizes as yet.
The objective of the invention is to develop a kind of goose down fur product innovation, be used for people's warming dress ornament, to beautify people's life.
Accompanying drawing is at process flow sheet of the present invention.
The present invention includes the technology of goose down fur product and shortening goose down fur. Goose down fur is with the goose skinning during slaughtering, takes out the fur that big hair, bristle form by shortening.
The ripening process of goose down fur is as follows:
1. epilation: goose is butchered the back peeling, choose out, take out big hair, bristle from the back.
2. degreasing: remove degrease blood stains and impurity with chemical materials.
3. immersion: immersion is pulled out after 2-3 hour and is extruded into water content 30-35% in temperature 30-40 ℃ water.
4. soak nitre:
Whole solution is 100%
Wherein: anhydrous sodium sulphate 5-6%
66 ° of B 0.08-0.15% of sulfuric acid
Wetting agent JFC 0.08-0.1%
Temperature 35-38 ℃
Time 24-30 hour.
Operating process is put into the container that above-mentioned solution is housed one by one to the goose down skin, and the wet pelt coefficient ratio of liquid and water content is 10: 1, and bubble evenly stirred once in 3 hours.
5. paste shovel: in order to make the dermatotome infiltration evenly, skin is pulled out, the water shovel is stepped on flat fleshing.
6. shortening: whole solution is 100%
Wherein: anhydrous sodium sulphate 6-8%,
Sodium-chlor 5-6%,
Chromium sulphate 0.1-0.15%,
Lead sulfate 0.2-0.25%,
Fossil meal 7-9%,
Temperature 35-38 ℃,
Time 68-80 hour.
7. oven dry: in kiln inner drying or seasoning.Dermatotome upwards is laid on the level land, and during to water content 20-25%, dermatotome closes dermatotome and accepted vexed 15-20 hour.
8. stuffing: emulsifying agent 10-15% is brushed in dermatotome after with the dilution of 35-40 ℃ of warm water, behind the vexed 10-20 clock, rub half an hour, maybe will play skin oil and heat and to 60-70 ℃ of dilution, brush, rub half an hour after vexed 10-20 minute in dermatotome with kneading machine.
9. perching.
10. dedusting decontamination dirt with dry-cleaning with trieline after the rotating cage lift-over, then becomes the pure white loose softish best product of splashing of fleece.
Embodiments of the invention are as follows:
One of the intact goose fur of degreasing, wet pelt heavily is 350 grams, after soaking one day with the clear water of 3.5Kg, the temperature that adds sodium sulfate 250 grams, sodium-chlor 200 grams, sulfuric acid 2.5CC, water was soaked 25 hours for 35 ℃, pull out with step on shovel meat after, in original solution, add chromium sulphate 4 grams, lead sulfate 8 grams, fossil meal 250 grams again, heat to 37 ℃, skin is dropped in the solution go out skin after 72 hours, dry, perching is product after the dedusting.
Advantage of the present invention:
1. the goose down fur product through shortening processing has abundant fine hair, and thermal property is good.
2. fine hair is pure white, dermatotome is soft, and outward appearance is good.
The plate light weight just, its tensile strength and pliability can compare favourably with animal skin.

Claims (2)

1, a kind of goose down fur is made up of dermatotome and fine hair, it is characterized in that it is that goose is butchered peeling, takes out big hair, and bristle is after the fur that shortening forms.
2, a kind of ripening process of goose down fur is characterized in that finishing through following step:
(1). epilation: goose is butchered the back peeling, take out big hair, bristle;
(2). degreasing: remove degrease, blood stains and impurity;
(3). immersion: immersion is pulled out after 2-3 hour and is extruded into water content 30-35% in temperature 30-40 ℃ water;
(4). soak nitre: whole solution is 100%;
Wherein: anhydrous sodium sulphate 5-6%,
Sulfuric acid 66B 0.08-0.15%,
Wetting agent JFC 0.08-0.1%,
Temperature 35-38 ℃,
Time 24-30 hour.
(5). paste shovel: skin is pulled out, and the water shovel is stepped on flat fleshing;
(6). shortening: whole solution is 100%;
Wherein: anhydrous sodium sulphate 6-8%,
Sodium-chlor 5-6%,
Chromium sulphate 0.1-0.15%,
Lead sulfate 0.2-0.25%,
Fossil meal 7-9%,
Temperature 35-38 ℃,
Time 68-80 hour.
(7). oven dry: in kiln inner drying or seasoning.Dermatotome upwards is laid on the level land, and during to water content 20-25%, dermatotome closes dermatotome and accepted vexed 15-20 hour.
(8). stuffing: emulsifying agent 10-15% is brushed in dermatotome after with the dilution of 35-40 ℃ of warm water, behind the vexed 10-20 clock, rub half an hour, maybe will play skin oil and heat and brush in dermatotome after the 60-70 ℃ of dilution, rub half an hour after vexed 10-20 minute.
(9). perching.
(10). dedusting: with using trieline dry washing cleaning dirt after the rotating cage lift-over.
CN 89105111 1989-06-20 1989-06-20 Goose down fur and ripening process thereof Pending CN1048234A (en)