CN103831172B - Method for improving antimony, lead and associated silver flotation recovery rate by adopting combination collecting agent - Google Patents

Method for improving antimony, lead and associated silver flotation recovery rate by adopting combination collecting agent Download PDF

Info

Publication number
CN103831172B
CN103831172B CN201410121821.0A CN201410121821A CN103831172B CN 103831172 B CN103831172 B CN 103831172B CN 201410121821 A CN201410121821 A CN 201410121821A CN 103831172 B CN103831172 B CN 103831172B
Authority
CN
China
Prior art keywords
antimony
collecting agent
lead
black powder
aerofloat
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Active
Application number
CN201410121821.0A
Other languages
Chinese (zh)
Other versions
CN103831172A (en
Inventor
刘建军
丁大森
欧阳金德
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Lhasa Weizhuo Rock And Mineral Analysis & Testing Co Ltd
TIBET HUAYU MINING Co Ltd
Original Assignee
Lhasa Weizhuo Rock And Mineral Analysis & Testing Co Ltd
TIBET HUAYU MINING Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Lhasa Weizhuo Rock And Mineral Analysis & Testing Co Ltd, TIBET HUAYU MINING Co Ltd filed Critical Lhasa Weizhuo Rock And Mineral Analysis & Testing Co Ltd
Priority to CN201410121821.0A priority Critical patent/CN103831172B/en
Publication of CN103831172A publication Critical patent/CN103831172A/en
Application granted granted Critical
Publication of CN103831172B publication Critical patent/CN103831172B/en
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

The invention relates to a method for increasing the flotation recovery of antimonial lead and associated silver by adopting a combination collecting agent. The combination collecting agent is composed of amyl sodium xanthate, 25 # black powder and butyl ammonium black powder; the weight ratio of the amyl sodium xanthate, the 25 # black powder and the butyl ammonium black powder is 2-5:20-35:15-30. By the adoption of the combination collecting agent, the antimony lead and associated silver flotation recovery rate can be greatly increased during flotation, the antimony and lead recovery rate is kept above 49% and can reach 59.09%, the lead recovery rate can reach 94.44%, the antimony recovery rate can reach 65.78%, the silver recovery rate can reach 88.31%, and the effect is obvious. In addition, the combination collecting agent can be adopted for operation under the situation that an original production technology is not changed, agentia is easy to add, the use rate of mineral resources is greatly increased, and the non-poisonous and non-pollution effect is achieved.

Description

A kind of method adopting combined capturing and collecting agent to improve antimony lead and associated silver flotation recovery rate
Technical field
The present invention relates to flotation from plumbous zinc antimony many metals raw ore and reclaim antimony lead and associated silver; The present invention be more particularly directed to a kind of method adopting combined capturing and collecting agent to improve antimony lead and associated silver flotation recovery rate.
Background technology
Sangri then mining area is positioned at Tibet Autonomous Region Longzi County, is the plumbous zinc multi-metal complex sulphide ore base of ultra-large type that Tibet Autonomous Region finds up to now; In this region, the embedding cloth relation of plumbous zinc many metals raw ore is complicated, and granule size thickness is uneven, belongs to complex refractory ore.In ore, main antimony mineral is boulangerite, jamesonite, and galena, stibnite are few; Zinc mineral is mainly zincblende; Silver mineral is mainly silver-colored antimony tetrahedrite.Jamesonite, boulangerite have corrosion in various degree to hand over phenomenon to galena, zincblende, pyrite, monomer dissociation difficulty, therefore current output lead antimony compound refined mine and zinc concentrate.
Along with mineral resources are exploited in a large number, poor, thin, assorted is the main feature of the tcrude ore resource of current exploitation.In this raw ore, jamesonite is compared with galena, have the advantages that disseminated grain size is thin, floatability is poor, and silver mineral is except main silver-colored antimony tetrahedrite, the main carriers mineral of other associated silver are boulangerite, jamesonite and galena etc., therefore effectively improve antimony, the plumbum floatation rate of recovery is the Important Action that associated silver is reclaimed in strengthening.Lot of experiments Researching and practicing shows, in this raw ore, boulangerite, jamesonite are to flotation pH value sensitivity, and experimental study is consistent with production practices to be shown, this raw ore of flotation is more suitable under the condition of neutral pH=7.0 ~ 7.5, and plumbous antimony flotation recovery rate is higher ;owing to containing a certain amount of zinc mineral in raw ore, therefore collector dosage strengthening collecting effect can not infinitely be strengthened in preferential floating plumbous antimony operation, say again, if excessive collecting agent pours in the selected operation of plumbous antimony, its lead-antimony concentrate grade is by uncontrollable, and lead adds antimony grade cannot remain on more than 45%, so not only affect Business Economic Benefit, too increase Product transport cost, directly have influence on the economic benefit of downstream smelting enterprise simultaneously.
Such as application number is 201010614789.1, publication number is the Chinese invention patent " a kind of method improving argillization high-sulfur jamesonite Floatation Concentrate Grade " of CN102218375A, which disclose a kind of method improving argillization high-sulfur jamesonite Floatation Concentrate Grade, the method needs, by adding the specific inhibitors such as tannin extract, to improve lead-antimony concentrate grade; Cause floatation process step complicated, and cost of investment is high; And the lead floatingly selected adds that antimony grade is the highest can only arrive 48.03%, lead adds that antimony recovery is the highest can only arrive 77.34%.
Such as application number is 201310413919.9 again, publication number is the Chinese invention patent " method for floating of the complicated jamesonite of a kind of microfine " of CN103433142A, which disclose the method for floating of the complicated jamesonite of a kind of microfine, comprise that carbon lead is separated, plumbous mud is separated, plumbous sulphur content from; The method needs to adopt special separating technology to obtain product; Special separating technology causes flotation cost of investment high, and the lead floatingly selected adds that antimony grade is the highest can only arrive 43.5%, and lead adds that antimony recovery is the highest can only arrive 66.12%.
Summary of the invention
The object of the invention is to the problems referred to above overcoming prior art existence, propose a kind of method adopting combined capturing and collecting agent to improve antimony lead and associated silver flotation recovery rate.It is under the condition of 7 ~ 7.5 that the present invention can be applicable to slurry pH, using zinc sulfate and sodium sulfite as zinc sulphide and pyritous inhibitor, then adds combined capturing and collecting agent; The flotation recovery rate of antimony lead and associated silver can be made in flotation to increase substantially, and lead adds antimony grade and remains on more than 49%, and lead adds antimony grade can reach 59.09%, and lead recovery can reach 94.44%, antimony recovery can reach 65.78%, silver raising recovery rate 88.31%, Be very effective; The present invention adopts combined capturing and collecting agent can operate when not changing original production technology, and medicament adds easy to implement, substantially increases Utilization Rate of Mineral Resources, and nontoxic pollution-free.
The present invention realizes by the following technical solutions:
A kind of combined capturing and collecting agent, is characterized in that: comprise amyl group sodium xanthate, 25 #black powder and aerofloat 226; Described amyl group sodium xanthate, 25 #the part by weight of black powder and aerofloat 226 is: 2 ~ 5:20 ~ 35:15 ~ 30.
During use, respectively amyl group sodium xanthate and aerofloat 226 are mixed with the aqueous solution that weight percent concentration is 1 ~ 5%, and 25 #black powder is stoste; Amyl group sodium acrinol solution, 25 #black powder stoste and the aerofloat 226 aqueous solution are for add in ore pulp respectively simultaneously.
Adopt combined capturing and collecting agent to improve a method for antimony lead and associated silver flotation recovery rate, it is characterized in that the method comprises the steps:
A, fragmentation, ore grinding:
By plumbous zinc antimony many metals raw ore after fragmentation, being ground to mineral disaggregation, form ore pulp;
B, flotation:
First in ore pulp, add the zinc sulfate suppressing zinc, sulfur mineral in ore pulp and sodium sulfite, after fully stirring; Add the combined capturing and collecting agent carrying out combining collecting to galena, jamesonite, stibnite, silver-colored antimony tetrahedrite and associated silver mineral again, combination collecting obtains lead-antimony concentrate product.By 25 in floatation process #black powder, amyl group sodium xanthate and aerofloat 226 add in ore pulp used in combination simultaneously respectively, can give full play to the cooperative effect between medicament.
Zinc sulfate and sodium sulfite are as the inhibitor of zinc, sulfur mineral; In combined capturing and collecting agent 25 #black powder and amyl group sodium xanthate are as the collecting agent of galena, jamesonite and stibnite, and aerofloat 226 is as the collecting agent of silver-colored antimony tetrahedrite and associated silver mineral.
By 1 ton of plumbous zinc antimony many metals raw ore, during flotation: zinc sulfate consumption is 400 ~ 1100g, sodium sulfite
Consumption is 90 ~ 180g, and combined capturing and collecting agent consumption is 370 ~ 700g.
During use, respectively zinc sulfate and sodium sulfite are mixed with the aqueous solution that weight percent concentration is 5 ~ 10%, more respectively amyl group sodium xanthate and aerofloat 226 are mixed with the aqueous solution that weight percent concentration is 1 ~ 5%, and 25 #black powder is stoste; First in ore pulp, add the zinc sulfate solution suppressing zinc, sulfur mineral and sodium sulfite aqueous solution, after fully stirring; Add the amyl group sodium acrinol solution, 25 carrying out combining collecting to galena, jamesonite, stibnite, silver-colored antimony tetrahedrite and associated silver mineral more respectively in ore pulp simultaneously #black powder stoste and the aerofloat 226 aqueous solution, combination collecting obtains lead-antimony concentrate product.
Add respectively refers at one time simultaneously, is joined by amyl group sodium acrinol solution separately in ore pulp, separately by 25 #black powder stoste joins in ore pulp He separately and is joined in ore pulp by the aerofloat 226 aqueous solution.
Amyl group sodium xanthate, 25 in described combined capturing and collecting agent #the part by weight of black powder and aerofloat 226 is: 23:306:157.
Amyl group sodium xanthate, 25 in described combined capturing and collecting agent #the part by weight of black powder and aerofloat 226 is: 28:266:197.
Amyl group sodium xanthate, 25 in described combined capturing and collecting agent #the part by weight of black powder and aerofloat 226 is: 35:237:219.
Described fragmentation refers to the fine ore plumbous zinc antimony many metals raw ore being crushed to granularity and being less than 12 millimeters; After described grinding refers to that the fine ore adopting ore mill granularity to be less than 12 millimeters is ground to mineral disaggregation, forming pH value is the ore pulp of 7 ~ 7.5.
25 #black powder is the conventional collecting agent of the sulphide ores such as lead, copper, silver.
Compared with prior art, its advantage is in the present invention:
1, the present invention can be applicable to slurry pH is under the condition of 7 ~ 7.5, using zinc sulfate and sodium sulfite as zinc sulphide and pyritous inhibitor, then adds combined capturing and collecting agent; The flotation recovery rate of antimony lead and associated silver can be made in flotation to increase substantially, and lead adds antimony grade and remains on more than 49%, and lead adds antimony grade can reach 59.09%, and lead recovery can reach 94.44%, antimony recovery can reach 65.78%, silver raising recovery rate 88.31%, Be very effective; The present invention adopts combined capturing and collecting agent can operate when not changing original production technology, and medicament adds easy to implement, substantially increases Utilization Rate of Mineral Resources, and nontoxic pollution-free.
2, the present invention is in use, and 25 #black powder is that stoste is added; Respectively amyl group sodium xanthate and aerofloat 226 are mixed with the aqueous solution, the aqueous solution of amyl group sodium xanthate 1 ~ 5% weight percent concentration; The aqueous solution of aerofloat 226 1 ~ 5% weight percent concentration; First amyl group sodium xanthate and aerofloat 226 are mixed with the aqueous solution, amyl group sodium acrinol solution and 25 #black powder can accelerate the reaction of galena in ore pulp, jamesonite and stibnite, strengthening collecting effect; Aerofloat 226 can accelerate the reaction of silver-colored antimony tetrahedrite and association silver ore in ore pulp, improves the ascent rate of silver-colored antimony tetrahedrite and association silver ore in ore pulp, thus improves collecting effect and the combination collecting rate of combined capturing and collecting agent.
3, medicament of the present invention is conventional dose, and medicament use amount is few, and cost is low, and nontoxic pollution-free; The application of the present invention scene is easy to implement; Can operate when not changing original production technology, avoiding and changing produced on-site technological process, cause that cost of investment is high, field conduct complicated situation occurs.
4, the present invention adopts 25 #black powder, amyl group sodium xanthate and aerofloat 226 combine rear interpolation in specific proportions, and concrete principle is: 25 #black powder and amyl group sodium xanthate are as the collecting agent of galena, jamesonite and stibnite, aerofloat 226 is as the collecting agent of silver-colored antimony tetrahedrite and association silver ore, the commerical test of 1 year 2500t/d has been carried out by above-mentioned technological parameter, result shows to adopt combinations thereof collecting agent dosage regimen effectively can carry the flotation recovery rate of high lead-antimony and associated silver, obtain lead-antimony concentrate: lead adds antimony grade and can reach and can reach 59.09%, lead recovery can reach 94.44%, antimony recovery can reach 65.78%, silver raising recovery rate 88.31%, Be very effective.
5, the present invention compared with prior art, do not need to add the adjusting agents such as large quantities of lime and remove deliberately to change pulp PH value, and the consumption of zinc sulfate and sodium sulfite is few, the lead adopting method of the present invention to floatingly select adds antimony grade can reach 59.09%, and lead recovery can reach 94.44%, antimony recovery can reach 65.78%, silver raising recovery rate 88.31%.
6, the present invention compares with " method for floating of the complicated jamesonite of a kind of microfine " with " a kind of method improving argillization high-sulfur jamesonite Floatation Concentrate Grade " in background technology, the present invention adopts conventional beneficiation reagent completely, and head adds zinc sulfate and sodium sulfite inhibitor zinc, sulfur mineral; Add again and comprise 25 #the combined capturing and collecting agent of black powder, amyl group sodium xanthate and aerofloat 226 carries out selective mixing collecting to target minreal; 25 #the part by weight of black powder, amyl group sodium xanthate and aerofloat 226 is: 2 ~ 5:20 ~ 35:15 ~ 30, make full use of 25 #black powder, cooperative effect between amyl group sodium xanthate and the interaction of aerofloat 226, reach the object of the flotation recovery rate improving antimony lead and associated silver; Lead adds antimony grade and improves 11.06% compared with employing existing " a kind of method improving argillization high-sulfur jamesonite Floatation Concentrate Grade "; Add antimony grade with adopting lead compared with existing " method for floating of the complicated jamesonite of a kind of microfine " and improve 15.59%; Be very effective of the present invention.
7, the present invention adopts amyl group sodium xanthate, 25 in described combined capturing and collecting agent #the part by weight of black powder and aerofloat 226 is: 23:306:157; The commerical test of 1 year 300t/d has been carried out by present invention process and combined capturing and collecting agent administration conditional parameter, result shows the flotation recovery rate effectively can putting forward high lead-antimony and associated silver, adopt one roughing, scan for three times, the plumbous antimony flow process of diffeential floatation that four times selected, flotation of lead antimony mine tailing flotation zinc again.Reach in the lead-antimony concentrate obtained in the ore pulp of 1.49% in leaded 3.15%, antimony 1.48%, zinc 3.75%, sulphur 5.73%, silver-colored 255.77g/t, carbon content: lead adds antimony grade 49.05%, argentiferous 3089.4g/t, lead recovery 78.42%, antimony recovery 64.82%, silver raising recovery rate 84.45%.
8, the present invention adopts amyl group sodium xanthate, 25 in described combined capturing and collecting agent #the part by weight of black powder and aerofloat 226 is: 28:266:197; The commerical test of 1 year 2000t/d has been carried out by present invention process and combined capturing and collecting agent administration conditional parameter, result shows the flotation recovery rate effectively can putting forward high lead-antimony and associated silver, adopt one roughing, scan for three times, the plumbous antimony flow process of diffeential floatation that four times selected, flotation of lead antimony mine tailing flotation zinc again.Reach in the lead-antimony concentrate obtained in the ore pulp of 1.52% in leaded 3.33%, antimony 1.05%, zinc 3.34%, sulphur 5.37%, silver-colored 163.45g/t, carbon content: lead adds antimony grade 59.09%, argentiferous 2257.16g/t, lead recovery 92.92%, antimony recovery 65.16%, silver raising recovery rate 88.31%.
9, the present invention adopts amyl group sodium xanthate, 25 in described combined capturing and collecting agent #the part by weight of black powder and aerofloat 226 is: 35:237:219; The commerical test of 1 year 2500t/d has been carried out by present invention process and combined capturing and collecting agent administration conditional parameter, result shows the flotation recovery rate effectively can putting forward high lead-antimony and associated silver, adopt one roughing, scan for three times, the plumbous antimony flow process of diffeential floatation that four times selected, flotation of lead antimony mine tailing flotation zinc again.Reach in the lead-antimony concentrate obtained in the ore pulp of 1.61% in leaded 3.15%, antimony 0.94%, zinc 3.21%, sulphur 5.57%, silver-colored 144.17g/t, carbon content: lead adds antimony grade 56.89%, argentiferous 2010.75g/t, lead recovery 94.44%, antimony recovery 65.78%, silver raising recovery rate 88.09%.
10, the present invention adopts 25 #black powder and amyl group sodium xanthate, as the collecting agent of galena, jamesonite and stibnite, make antimony lead lock out operation steady, and aerofloat 226, as the collecting agent of silver-colored antimony tetrahedrite and associated silver mineral, makes silver-colored lock out operation steady; And 25 #black powder, cooperative effect between amyl group sodium xanthate and the interaction of aerofloat 226, can also improve the flotation recovery rate of antimony lead and associated silver.
Detailed description of the invention
Below by way of concrete example of implementing, technical scheme of the present invention is further described.
Embodiment 1:
A kind of combined capturing and collecting agent, comprises amyl group sodium xanthate, 25 #black powder and aerofloat 226; Described amyl group sodium xanthate, 25 #the part by weight of black powder and aerofloat 226 is: 23:306:157.
During use, respectively amyl group sodium xanthate and aerofloat 226 are mixed with the aqueous solution that weight percent concentration is 2.5%, and 25 #black powder is stoste; Amyl group sodium acrinol solution, 25 #black powder stoste and the aerofloat 226 aqueous solution are for add in ore pulp respectively simultaneously.
The present invention is applied in a kind of combined capturing and collecting agent that adopts and improves in the method for antimony lead and associated silver flotation recovery rate, and the method comprises the steps:
A, fragmentation, ore grinding:
By plumbous zinc antimony many metals raw ore after fragmentation, being ground to mineral disaggregation, form ore pulp;
B, flotation:
First in ore pulp, add the zinc sulfate suppressing zinc, sulfur mineral in ore pulp and sodium sulfite, after fully stirring; Add the combined capturing and collecting agent carrying out combining collecting to galena, jamesonite, stibnite, silver-colored antimony tetrahedrite and associated silver mineral again, combination collecting obtains lead-antimony concentrate product.
Described fragmentation refers to the fine ore plumbous zinc antimony many metals raw ore being crushed to granularity and being less than 12 millimeters; After described grinding refers to that the fine ore adopting ore mill granularity to be less than 12 millimeters is ground to mineral disaggregation, forming pH value is the ore pulp of 7 ~ 7.5.
Zinc sulfate and sodium sulfite are as the inhibitor of zinc, sulfur mineral; In combined capturing and collecting agent 25 #black powder and amyl group sodium xanthate are as the collecting agent of galena, jamesonite and stibnite, and aerofloat 226 is as the collecting agent of silver-colored antimony tetrahedrite and associated silver mineral.
The present invention is when embody rule:
1, plumbous zinc antimony many metal raw mineral material:
In the ore pulp formed: leaded 3.15%, antimony 1.48%, zinc 3.75%, sulphur 5.73%, silver-colored 255.77g/t, carbon content reach 1.49%; Pulp density 39.54%, fineness-74 microns of grades account for 80.85%; Plumbous antimony mainly exists with boulangerite and jamesonite form, and zinc is based on zincblende, and sulphur is based on pyrite and mispickel, and phosphorus content is higher, and fine particle stage material is than great.
2, floating agent and operating procedure:
Regime of agent:
By 1 ton of plumbous zinc antimony many metals raw ore, in flotation: zinc sulfate consumption is 1057g, sodium sulfite consumption is 155g, and amyl group sodium xanthate consumption is 23g, 25 #black powder consumption is 306g, and aerofloat 226 consumption is 157g.
During use, first medicament is mixed with following weight percent concentration:
Zinc sulfate 5% aqueous solution
Sodium sulfite 5% aqueous solution
Amyl group sodium xanthate 2.5% aqueous solution
25 #black powder stoste is added
Aerofloat 226 2.5% aqueous solution;
Operating procedure:
After fragmentation, regrind plumbous zinc antimony many metals raw ore to fineness-74 microns of grades account for 80.85%, weight concentration is the ore pulp of 39.54%; First add toward ore pulp in and suppress zincblende and pyritous zinc sulfate solution and sodium sulfite aqueous solution, fully after stirring; Add the amyl group sodium acrinol solution, 25 carrying out combining collecting to galena, jamesonite, stibnite, silver-colored antimony tetrahedrite and associated silver mineral more respectively in ore pulp simultaneously #black powder stoste and the aerofloat 226 aqueous solution, combination collecting obtains lead-antimony concentrate product.
The commerical test of 1 year 300t/d has been carried out by above-mentioned technological parameter, result shows to adopt above-mentioned technique and combined capturing and collecting agent administration condition effectively can carry the flotation recovery rate of high lead-antimony and associated silver, adopt one roughing, scan for three times, the plumbous antimony flow process of diffeential floatation that four times selected, flotation of lead antimony mine tailing flotation zinc again.Reach in the lead-antimony concentrate obtained in the ore pulp of 1.49% in leaded 3.15%, antimony 1.48%, zinc 3.75%, sulphur 5.73%, silver-colored 255.77g/t, carbon content: lead adds antimony grade 49.05%, argentiferous 3089.4g/t, lead recovery 78.42%, antimony recovery 64.82%, silver raising recovery rate 84.45%.
Embodiment 2:
A kind of combined capturing and collecting agent, comprises amyl group sodium xanthate, 25 #black powder and aerofloat 226; Described amyl group sodium xanthate, 25 #the part by weight of black powder and aerofloat 226 is: 28:266:197.
During use, respectively amyl group sodium xanthate and aerofloat 226 are mixed with the aqueous solution that weight percent concentration is 2.5%, and 25 #black powder is stoste; Amyl group sodium acrinol solution, 25 #black powder stoste and the aerofloat 226 aqueous solution are for add in ore pulp respectively simultaneously.
The present invention is applied in a kind of combined capturing and collecting agent that adopts and improves in the method for antimony lead and associated silver flotation recovery rate, and the method comprises the steps:
A, fragmentation, ore grinding:
By plumbous zinc antimony many metals raw ore after fragmentation, being ground to mineral disaggregation, form ore pulp;
B, flotation:
First in ore pulp, add the zinc sulfate suppressing zinc, sulfur mineral in ore pulp and sodium sulfite, after fully stirring; Add the combined capturing and collecting agent carrying out combining collecting to galena, jamesonite, stibnite, silver-colored antimony tetrahedrite and associated silver mineral again, combination collecting obtains lead-antimony concentrate product.
Described fragmentation refers to the fine ore plumbous zinc antimony many metals raw ore being crushed to granularity and being less than 12 millimeters; After described grinding refers to that the fine ore adopting ore mill granularity to be less than 12 millimeters is ground to mineral disaggregation, forming pH value is the ore pulp of 7 ~ 7.5.
Zinc sulfate and sodium sulfite are as the inhibitor of zinc, sulfur mineral; In combined capturing and collecting agent 25 #black powder and amyl group sodium xanthate are as the collecting agent of galena, jamesonite and stibnite, and aerofloat 226 is as the collecting agent of silver-colored antimony tetrahedrite and associated silver mineral.
The present invention is when embody rule:
1, plumbous zinc antimony many metal raw mineral material:
In the ore pulp formed: leaded 3.33%, antimony 1.05%, zinc 3.34%, sulphur 5.37%, silver-colored 163.45g/t, carbon content reach 1.52%; Pulp density 38.79%, fineness-74 microns of grades account for 81.44%; Plumbous antimony mainly exists with boulangerite and jamesonite form, and zinc is based on zincblende, and sulphur is based on pyrite and mispickel, and phosphorus content is higher, and fine particle stage material is than great.
2, floating agent and operating procedure:
Regime of agent:
By 1 ton of plumbous zinc antimony many metals raw ore, in flotation: zinc sulfate consumption is 864g, sodium sulfite consumption is 178g, and amyl group sodium xanthate consumption is 28g, 25 #black powder consumption is 266g, and aerofloat 226 consumption is 197g.
During use, first medicament is mixed with following weight percent concentration:
Zinc sulfate 5% aqueous solution
Sodium sulfite 5% aqueous solution
Amyl group sodium xanthate 2.5% aqueous solution
25 #black powder stoste is added
Aerofloat 226 2.5% aqueous solution;
Operating procedure:
First after fragmentation, regrind plumbous zinc antimony many metals raw ore to fineness-74 microns of grades and account for 81.44%, weight concentration is the ore pulp of 38.79%; First add toward ore pulp in and suppress zincblende and pyritous zinc sulfate solution and sodium sulfite aqueous solution, fully after stirring; Add the amyl group sodium acrinol solution, 25 carrying out combining collecting to galena, jamesonite, stibnite, silver-colored antimony tetrahedrite and associated silver mineral more respectively in ore pulp simultaneously #black powder stoste and the aerofloat 226 aqueous solution, combination collecting obtains lead-antimony concentrate product.
The commerical test of 1 year 2000t/d has been carried out by above-mentioned technological parameter, result shows to adopt above-mentioned technique and combined capturing and collecting agent administration condition effectively can carry the flotation recovery rate of high lead-antimony and associated silver, adopt one roughing, scan for three times, the plumbous antimony flow process of diffeential floatation that four times selected, flotation of lead antimony mine tailing flotation zinc again.Reach in the lead-antimony concentrate obtained in the ore pulp of 1.52% in leaded 3.33%, antimony 1.05%, zinc 3.34%, sulphur 5.37%, silver-colored 163.45g/t, carbon content: lead adds antimony grade 59.09%, argentiferous 2257.16g/t, lead recovery 92.92%, antimony recovery 65.16%, silver raising recovery rate 88.31%.This embodiment is most preferred embodiment of the present invention.
Embodiment 3:
A kind of combined capturing and collecting agent, comprises amyl group sodium xanthate, 25 #black powder and aerofloat 226; Described amyl group sodium xanthate, 25 #the part by weight of black powder and aerofloat 226 is: 35:237:219.
During use, respectively amyl group sodium xanthate and aerofloat 226 are mixed with the aqueous solution that weight percent concentration is 2.5%, and 25 #black powder is stoste; Amyl group sodium acrinol solution, 25 #black powder stoste and the aerofloat 226 aqueous solution are for add in ore pulp respectively simultaneously.
The present invention is applied in a kind of combined capturing and collecting agent that adopts and improves in the method for antimony lead and associated silver flotation recovery rate, and the method comprises the steps:
A, fragmentation, ore grinding:
By plumbous zinc antimony many metals raw ore after fragmentation, being ground to mineral disaggregation, form ore pulp;
B, flotation:
First in ore pulp, add the zinc sulfate suppressing zinc, sulfur mineral in ore pulp and sodium sulfite, after fully stirring; Add the combined capturing and collecting agent carrying out combining collecting to galena, jamesonite, stibnite, silver-colored antimony tetrahedrite and associated silver mineral again, combination collecting obtains lead-antimony concentrate product.
Described fragmentation refers to the fine ore plumbous zinc antimony many metals raw ore being crushed to granularity and being less than 12 millimeters; After described grinding refers to that the fine ore adopting ore mill granularity to be less than 12 millimeters is ground to mineral disaggregation, forming pH value is the ore pulp of 7 ~ 7.5.
Zinc sulfate and sodium sulfite are as the inhibitor of zinc, sulfur mineral; In combined capturing and collecting agent 25 #black powder and amyl group sodium xanthate are as the collecting agent of galena, jamesonite and stibnite, and aerofloat 226 is as the collecting agent of silver-colored antimony tetrahedrite and associated silver mineral.
The present invention is when embody rule:
1, plumbous zinc antimony many metal raw mineral material:
In the ore pulp formed: leaded 3.15%, antimony 0.94%, zinc 3.21%, sulphur 5.57%, silver-colored 144.17g/t, carbon content reach 1.61%; Pulp density 38.26%, fineness-74 microns of grades account for 81.73%; Plumbous antimony mainly exists with boulangerite and jamesonite form, and zinc is based on zincblende, and sulphur is based on pyrite and mispickel, and phosphorus content is higher, and fine particle stage material is than great.
2, floating agent and operating procedure:
Regime of agent:
By 1 ton of plumbous zinc antimony many metals raw ore, in flotation: zinc sulfate consumption is 753g, sodium sulfite consumption is 165g, and amyl group sodium xanthate consumption is 35g, 25 #black powder consumption is 237g, and aerofloat 226 consumption is 219g.
During use, first medicament is mixed with following weight percent concentration:
Zinc sulfate 5% aqueous solution
Sodium sulfite 5% aqueous solution
Amyl group sodium xanthate 2.5% aqueous solution
25 #black powder stoste is added
Aerofloat 226 2.5% aqueous solution;
Operating procedure:
First after fragmentation, regrind plumbous zinc antimony many metals raw ore to fineness-74 microns of grades and account for 810.73%, weight concentration is the ore pulp of 38.26%; First add toward ore pulp in and suppress zincblende and pyritous zinc sulfate solution and sodium sulfite aqueous solution, fully after stirring; Add the amyl group sodium acrinol solution, 25 carrying out combining collecting to galena, jamesonite, stibnite, silver-colored antimony tetrahedrite and associated silver mineral more respectively in ore pulp simultaneously #black powder stoste and the aerofloat 226 aqueous solution, combination collecting obtains lead-antimony concentrate product.
The commerical test of 1 year 2500t/d has been carried out by above-mentioned technological parameter, result shows to adopt above-mentioned technique and combined capturing and collecting agent administration condition effectively can carry the flotation recovery rate of high lead-antimony and associated silver, adopt one roughing, scan for three times, the plumbous antimony flow process of diffeential floatation that four times selected, flotation of lead antimony mine tailing flotation zinc again.Reach in the lead-antimony concentrate obtained in the ore pulp of 1.61% in leaded 3.15%, antimony 0.94%, zinc 3.21%, sulphur 5.57%, silver-colored 144.17g/t, carbon content: lead adds antimony grade 56.89%, argentiferous 2010.75g/t, lead recovery 94.44%, antimony recovery 65.78%, silver raising recovery rate 88.09%.
Embodiment 4:
A kind of combined capturing and collecting agent, comprises amyl group sodium xanthate, 25 #black powder and aerofloat 226; Described amyl group sodium xanthate, 25 #the part by weight of black powder and aerofloat 226 is: 20:200:150.
During use, respectively amyl group sodium xanthate and aerofloat 226 are mixed with the aqueous solution that weight percent concentration is 5%, and 25 #black powder is stoste; Amyl group sodium acrinol solution, 25 #black powder stoste and the aerofloat 226 aqueous solution are for add in ore pulp respectively simultaneously.
The present invention is applied in a kind of combined capturing and collecting agent that adopts and improves in the method for antimony lead and associated silver flotation recovery rate, and the method comprises the steps:
A, fragmentation, ore grinding:
By plumbous zinc antimony many metals raw ore after fragmentation, being ground to mineral disaggregation, form ore pulp;
B, flotation:
First in ore pulp, add the zinc sulfate suppressing zinc, sulfur mineral in ore pulp and sodium sulfite, after fully stirring; Add the combined capturing and collecting agent carrying out combining collecting to galena, jamesonite, stibnite, silver-colored antimony tetrahedrite and associated silver mineral again, combination collecting obtains lead-antimony concentrate product.
Described fragmentation refers to the fine ore plumbous zinc antimony many metals raw ore being crushed to granularity and being less than 12 millimeters; After described grinding refers to that the fine ore adopting ore mill granularity to be less than 12 millimeters is ground to mineral disaggregation, forming pH value is the ore pulp of 7 ~ 7.5.
Zinc sulfate and sodium sulfite are as the inhibitor of zinc, sulfur mineral; In combined capturing and collecting agent 25 #black powder and amyl group sodium xanthate are as the collecting agent of galena, jamesonite and stibnite, and aerofloat 226 is as the collecting agent of silver-colored antimony tetrahedrite and associated silver mineral.
The present invention is when embody rule:
1, plumbous zinc antimony many metal raw mineral material:
In the ore pulp formed: leaded 3.15%, antimony 1.48%, zinc 3.75%, sulphur 5.73%, silver-colored 255.77g/t, carbon content reach 1.49%; Pulp density 39.54%, fineness-74 microns of grades account for 80.85%; Plumbous antimony mainly exists with boulangerite and jamesonite form, and zinc is based on zincblende, and sulphur is based on pyrite and mispickel, and phosphorus content is higher, and fine particle stage material is than great.
2, floating agent and operating procedure:
Regime of agent:
By 1 ton of plumbous zinc antimony many metals raw ore, in flotation: zinc sulfate consumption is 400g, sodium sulfite consumption is 90g, and amyl group sodium xanthate consumption is 20g, 25 #black powder consumption is 200g, and aerofloat 226 consumption is 150g.
During use, first medicament is mixed with following weight percent concentration:
Zinc sulfate 10% aqueous solution
Sodium sulfite 10% aqueous solution
Amyl group sodium xanthate 5% aqueous solution
25 #black powder stoste is added
Aerofloat 226 5% aqueous solution;
Operating procedure:
First after fragmentation, regrind plumbous zinc antimony many metals raw ore to fineness-74 microns of grades and account for 80.85%, weight concentration is the ore pulp of 39.54%; First add toward ore pulp in and suppress zincblende and pyritous zinc sulfate solution and sodium sulfite aqueous solution, fully after stirring; Add the amyl group sodium acrinol solution, 25 carrying out combining collecting to galena, jamesonite, stibnite, silver-colored antimony tetrahedrite and associated silver mineral more respectively in ore pulp simultaneously #black powder stoste and the aerofloat 226 aqueous solution, combination collecting obtains lead-antimony concentrate product.
The commerical test of 1 year 300t/d has been carried out by above-mentioned technological parameter, result shows to adopt above-mentioned technique and combined capturing and collecting agent administration condition effectively can carry the flotation recovery rate of high lead-antimony and associated silver, adopt one roughing, scan for three times, the plumbous antimony flow process of diffeential floatation that four times selected, flotation of lead antimony mine tailing flotation zinc again.Reach in the lead-antimony concentrate obtained in the ore pulp of 1.49% in leaded 3.15%, antimony 1.48%, zinc 3.75%, sulphur 5.73%, silver-colored 255.77g/t, carbon content: lead adds antimony grade 49.01%, argentiferous 3055.3g/t, lead recovery 78.15%, antimony recovery 64.44%, silver raising recovery rate 84.08%.
Embodiment 5:
A kind of combined capturing and collecting agent, comprises amyl group sodium xanthate, 25 #black powder and aerofloat 226; Described amyl group sodium xanthate, 25 #the part by weight of black powder and aerofloat 226 is: 21:250:190.
During use, respectively amyl group sodium xanthate and aerofloat 226 are mixed with the aqueous solution that weight percent concentration is 2.5%, and 25 #black powder is stoste; Amyl group sodium acrinol solution, 25 #black powder stoste and the aerofloat 226 aqueous solution are for add in ore pulp respectively simultaneously.
The present invention is applied in a kind of combined capturing and collecting agent that adopts and improves in the method for antimony lead and associated silver flotation recovery rate, and the method comprises the steps:
A, fragmentation, ore grinding:
By plumbous zinc antimony many metals raw ore after fragmentation, being ground to mineral disaggregation, form ore pulp;
B, flotation:
First in ore pulp, add the zinc sulfate suppressing zinc, sulfur mineral in ore pulp and sodium sulfite, after fully stirring; Add the combined capturing and collecting agent carrying out combining collecting to galena, jamesonite, stibnite, silver-colored antimony tetrahedrite and associated silver mineral again, combination collecting obtains lead-antimony concentrate product.
Described fragmentation refers to the fine ore plumbous zinc antimony many metals raw ore being crushed to granularity and being less than 12 millimeters; After described grinding refers to that the fine ore adopting ore mill granularity to be less than 12 millimeters is ground to mineral disaggregation, forming pH value is the ore pulp of 7 ~ 7.5.
Zinc sulfate and sodium sulfite are as the inhibitor of zinc, sulfur mineral; In combined capturing and collecting agent 25 #black powder and amyl group sodium xanthate are as the collecting agent of galena, jamesonite and stibnite, and aerofloat 226 is as the collecting agent of silver-colored antimony tetrahedrite and associated silver mineral.
The present invention is when embody rule:
1, plumbous zinc antimony many metal raw mineral material:
In the ore pulp formed: leaded 3.15%, antimony 1.48%, zinc 3.75%, sulphur 5.73%, silver-colored 255.77g/t, carbon content reach 1.49%; Pulp density 39.54%, fineness-74 microns of grades account for 80.85%; Plumbous antimony mainly exists with boulangerite and jamesonite form, and zinc is based on zincblende, and sulphur is based on pyrite and mispickel, and phosphorus content is higher, and fine particle stage material is than great.
2, floating agent and operating procedure:
Regime of agent:
By 1 ton of plumbous zinc antimony many metals raw ore, in flotation: zinc sulfate consumption is 700g, sodium sulfite consumption is 120g, and amyl group sodium xanthate consumption is 21g, 25 #black powder consumption is 250g, and aerofloat 226 consumption is 190g.
During use, first medicament is mixed with following weight percent concentration:
Zinc sulfate 7% aqueous solution
Sodium sulfite 7% aqueous solution
Amyl group sodium xanthate 5% aqueous solution
25 #black powder stoste is added
Aerofloat 226 5% aqueous solution;
Operating procedure:
First after fragmentation, regrind plumbous zinc antimony many metals raw ore to fineness-74 microns of grades and account for 80.85%, weight concentration is the ore pulp of 39.54%; First add toward ore pulp in and suppress zincblende and pyritous zinc sulfate solution and sodium sulfite aqueous solution, fully after stirring; Add the amyl group sodium acrinol solution, 25 carrying out combining collecting to galena, jamesonite, stibnite, silver-colored antimony tetrahedrite and associated silver mineral more respectively in ore pulp simultaneously #black powder stoste and the aerofloat 226 aqueous solution, combination collecting obtains lead-antimony concentrate product.
The commerical test of 1 year 300t/d has been carried out by above-mentioned technological parameter, result shows to adopt above-mentioned technique and combined capturing and collecting agent administration condition effectively can carry the flotation recovery rate of high lead-antimony and associated silver, adopt one roughing, scan for three times, the plumbous antimony flow process of diffeential floatation that four times selected, flotation of lead antimony mine tailing flotation zinc again.Reach in the lead-antimony concentrate obtained in the ore pulp of 1.49% in leaded 3.15%, antimony 1.48%, zinc 3.75%, sulphur 5.73%, silver-colored 255.77g/t, carbon content: lead adds antimony grade 49.55%, argentiferous 3080.7g/t, lead recovery 78.66%, antimony recovery 65.09%, silver raising recovery rate 84.92%.
Embodiment 6:
A kind of combined capturing and collecting agent, comprises amyl group sodium xanthate, 25 #black powder and aerofloat 226; Described amyl group sodium xanthate, 25 #the part by weight of black powder and aerofloat 226 is: 50:350:300.
During use, respectively amyl group sodium xanthate and aerofloat 226 are mixed with the aqueous solution that weight percent concentration is 1%, and 25 #black powder is stoste; Amyl group sodium acrinol solution, 25 #black powder stoste and the aerofloat 226 aqueous solution are for add in ore pulp respectively simultaneously.
The present invention is applied in a kind of combined capturing and collecting agent that adopts and improves in the method for antimony lead and associated silver flotation recovery rate, and the method comprises the steps:
A, fragmentation, ore grinding:
By plumbous zinc antimony many metals raw ore after fragmentation, being ground to mineral disaggregation, form ore pulp;
B, flotation:
First in ore pulp, add the zinc sulfate suppressing zinc, sulfur mineral in ore pulp and sodium sulfite, after fully stirring; Add the combined capturing and collecting agent carrying out combining collecting to galena, jamesonite, stibnite, silver-colored antimony tetrahedrite and associated silver mineral again, combination collecting obtains lead-antimony concentrate product.
Described fragmentation refers to the fine ore plumbous zinc antimony many metals raw ore being crushed to granularity and being less than 12 millimeters; After described grinding refers to that the fine ore adopting ore mill granularity to be less than 12 millimeters is ground to mineral disaggregation, forming pH value is the ore pulp of 7 ~ 7.5.
Zinc sulfate and sodium sulfite are as the inhibitor of zinc, sulfur mineral; In combined capturing and collecting agent 25 #black powder and amyl group sodium xanthate are as the collecting agent of galena, jamesonite and stibnite, and aerofloat 226 is as the collecting agent of silver-colored antimony tetrahedrite and associated silver mineral.
The present invention is when embody rule:
1, plumbous zinc antimony many metal raw mineral material:
In the ore pulp formed: leaded 3.33%, antimony 1.05%, zinc 3.34%, sulphur 5.37%, silver-colored 163.45g/t, carbon content reach 1.52%; Pulp density 38.79%, fineness-74 microns of grades account for 81.44%; Plumbous antimony mainly exists with boulangerite and jamesonite form, and zinc is based on zincblende, and sulphur is based on pyrite and mispickel, and phosphorus content is higher, and fine particle stage material is than great.
2, floating agent and operating procedure:
Regime of agent:
By 1 ton of plumbous zinc antimony many metals raw ore, in flotation: zinc sulfate consumption is 1100g, sodium sulfite consumption is 180g, and amyl group sodium xanthate consumption is 50g, 25 #black powder consumption is 350g, and aerofloat 226 consumption is 300g.
During use, first medicament is mixed with following weight percent concentration:
Zinc sulfate 5% aqueous solution
Sodium sulfite 5% aqueous solution
Amyl group sodium xanthate 1% aqueous solution
25 #black powder stoste is added
Aerofloat 226 1% aqueous solution;
Operating procedure:
First after fragmentation, regrind plumbous zinc antimony many metals raw ore to fineness-74 microns of grades and account for 81.44%, weight concentration is the ore pulp of 38.79%; First add toward ore pulp in and suppress zincblende and pyritous zinc sulfate solution and sodium sulfite aqueous solution, fully after stirring; Add the amyl group sodium acrinol solution, 25 carrying out combining collecting to galena, jamesonite, stibnite, silver-colored antimony tetrahedrite and associated silver mineral more respectively in ore pulp simultaneously #black powder stoste and the aerofloat 226 aqueous solution, combination collecting obtains lead-antimony concentrate product.
The commerical test of 1 year 2000t/d has been carried out by above-mentioned technological parameter, result shows to adopt above-mentioned technique and combined capturing and collecting agent administration condition effectively can carry the flotation recovery rate of high lead-antimony and associated silver, adopt one roughing, scan for three times, the plumbous antimony flow process of diffeential floatation that four times selected, flotation of lead antimony mine tailing flotation zinc again.Reach in the lead-antimony concentrate obtained in the ore pulp of 1.52% in leaded 3.33%, antimony 1.05%, zinc 3.34%, sulphur 5.37%, silver-colored 163.45g/t, carbon content: lead adds antimony grade 58.55%, argentiferous 2202.16g/t, lead recovery 91.77%, antimony recovery 64.56%, silver raising recovery rate 87.49%.

Claims (6)

1. adopt combined capturing and collecting agent to improve a method for antimony lead and associated silver flotation recovery rate, it is characterized in that the method comprises the steps:
A, fragmentation, ore grinding:
By plumbous zinc antimony many metals raw ore after fragmentation, being ground to mineral disaggregation, form ore pulp;
B, flotation:
First in ore pulp, add the zinc sulfate suppressing zinc, sulfur mineral in ore pulp and sodium sulfite, after fully stirring; Add the combined capturing and collecting agent carrying out combining collecting to galena, jamesonite, stibnite, silver-colored antimony tetrahedrite and associated silver mineral again, combination collecting obtains lead-antimony concentrate product;
Combined capturing and collecting agent comprises amyl group sodium xanthate, 25 #black powder and aerofloat 226; Described amyl group sodium xanthate, 25 #the part by weight of black powder and aerofloat 226 is: 2 ~ 5:20 ~ 35:15 ~ 30; During use, respectively amyl group sodium xanthate and aerofloat 226 are mixed with the aqueous solution that weight percent concentration is 1 ~ 5%, and 25 #black powder is stoste; Amyl group sodium acrinol solution, 25 #black powder stoste and the aerofloat 226 aqueous solution are for add in ore pulp respectively simultaneously;
By 1 ton of plumbous zinc antimony many metals raw ore, during flotation: zinc sulfate consumption is 400 ~ 1100g, sodium sulfite consumption is 90 ~ 180g, and combined capturing and collecting agent consumption is 370 ~ 700g;
Described fragmentation refers to the fine ore plumbous zinc antimony many metals raw ore being crushed to granularity and being less than 12 millimeters; After described grinding refers to that the fine ore adopting ore mill granularity to be less than 12 millimeters is ground to mineral disaggregation, forming pH value is the ore pulp of 7 ~ 7.5.
2. a kind of method adopting combined capturing and collecting agent to improve antimony lead and associated silver flotation recovery rate according to claim 1, it is characterized in that: during use, respectively zinc sulfate and sodium sulfite are mixed with the aqueous solution that weight percent concentration is 5 ~ 10%, respectively amyl group sodium xanthate and aerofloat 226 are mixed with the aqueous solution that weight percent concentration is 1 ~ 5% again, and 25 #black powder is stoste; First in ore pulp, add the zinc sulfate solution suppressing zinc, sulfur mineral and sodium sulfite aqueous solution, after fully stirring; Add the amyl group sodium acrinol solution, 25 carrying out combining collecting to galena, jamesonite, stibnite, silver-colored antimony tetrahedrite and associated silver mineral more respectively in ore pulp simultaneously #black powder stoste and the aerofloat 226 aqueous solution, combination collecting obtains lead-antimony concentrate product.
3. a kind of method adopting combined capturing and collecting agent to improve antimony lead and associated silver flotation recovery rate according to claim 1, is characterized in that: zinc sulfate and sodium sulfite are as the inhibitor of zinc, sulfur mineral; 25 #black powder and amyl group sodium xanthate are as the collecting agent of galena, jamesonite and stibnite, and aerofloat 226 is as the collecting agent of silver-colored antimony tetrahedrite and associated silver mineral.
4. a kind of method adopting combined capturing and collecting agent to improve antimony lead and associated silver flotation recovery rate according to claim 1, is characterized in that: amyl group sodium xanthate, 25 in described combined capturing and collecting agent #the part by weight of black powder and aerofloat 226 is: 28:266:197.
5. a kind of method adopting combined capturing and collecting agent to improve antimony lead and associated silver flotation recovery rate according to claim 1, is characterized in that: amyl group sodium xanthate, 25 in described combined capturing and collecting agent #the part by weight of black powder and aerofloat 226 is: 23:306:157.
6. a kind of method adopting combined capturing and collecting agent to improve antimony lead and associated silver flotation recovery rate according to claim 1, is characterized in that: amyl group sodium xanthate, 25 in described combined capturing and collecting agent #the part by weight of black powder and aerofloat 226 is: 35:237:219.
CN201410121821.0A 2014-03-28 2014-03-28 Method for improving antimony, lead and associated silver flotation recovery rate by adopting combination collecting agent Active CN103831172B (en)