CN103820819A - Titanium mother board edge-binding method capable of controlling size of starting sheet - Google Patents
Titanium mother board edge-binding method capable of controlling size of starting sheet Download PDFInfo
- Publication number
- CN103820819A CN103820819A CN201410071087.1A CN201410071087A CN103820819A CN 103820819 A CN103820819 A CN 103820819A CN 201410071087 A CN201410071087 A CN 201410071087A CN 103820819 A CN103820819 A CN 103820819A
- Authority
- CN
- China
- Prior art keywords
- starting sheet
- bound edge
- titanium
- titanium starting
- edge
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Granted
Abstract
The invention provides a titanium mother board edge-binding method capable of controlling the size of a starting sheet. According to the starting sheet size requirement, besides edge-binding of two sides and bottom of the titanium mother board, the upper part of the titanium mother board is also edge-bound by pasting of an insulated rubber tape, opening of a dovetail groove and injection moulding, manual or screen printing of an insulating paint and the like. The method specifically comprises the following steps: determining the edge-binding position of the upper part of the titanium mother board, burnishing the edge-binding area, polishing, cleaning, and edge-binding the upper part of the titanium mother board. By edge-binding of the upper part of the titanium mother board, the size of the starting sheet can be controlled, edge shearing amount of the starting sheet can be reduced, and quality grade rate of a product can be raised.
Description
Technical field
The invention belongs to smelting field of nonferrous metal, relate to a kind of titanium starting sheet Wrapping method of controlling starting sheet size.
Background technology
In common nickel, electrolytic refining course of copper, adopt at present titanium starting sheet to produce starting sheet, and general titanium starting sheet is all large compared with starting sheet size, existing most smelting producers adopts variety of way and material to carry out bound edge in both sides and the bottom of titanium starting sheet, and bound edge is not carried out in the top of titanium starting sheet.And the starting sheet of producing all will be sheared by specification opposite side portion, if not bound edge of titanium starting sheet top, the starting sheet shearing displacement that the starting sheet top shearing displacement of producing carries out bound edge compared with top will increase, along with the increase of turnout, limit portion accumulative total shearing displacement increases, and can affect percentage of product or the utilization ratio of product.
Summary of the invention
The present invention is directed to the titanium starting sheet top using in above-mentioned nickel, the production of cupric electrolysis starting sheet and there is no bound edge, causing limit portion accumulative total shearing displacement to increase affects the percentage of product of product or the problem of utilization ratio, and a kind of method of bound edge control starting sheet specification in optimum range of carrying out on titanium starting sheet top is provided.
A titanium starting sheet Wrapping method of controlling starting sheet size, comprises the following steps
A) determine the position of titanium starting sheet top bound edge:
Determining of titanium starting sheet top bound edge width: titanium starting sheet top bound edge wide be on bound edge width along highly and under bound edge width along the difference between height, on described bound edge width, the height on edge is determined according to exceeding cathode compartment liquid level 20-50mm, and the height that under described bound edge width, the height on edge is starting sheet adds the height of titanium starting sheet bottom bound edge and the height of starting sheet top shearing surplus.
Determining of titanium starting sheet top bound edge length: the length of titanium starting sheet top bound edge and the width of titanium starting sheet are consistent;
B) pack processing edge regions: to bound edge region polish, polishing, cleaning;
C) bound edge of titanium starting sheet: the top of titanium starting sheet is adopted and pastes insulation tape or silk screen printing insulation compound or open dovetail-indent injection moulding mode and carry out bound edge.
In described step c, adopting the mode of stickup insulation tape bound edge is after completing steps a and b, insulation tape cuts, pastes and cover on titanium starting sheet according to the size in bound edge region, titanium starting sheet top, according to this method, the another side of titanium starting sheet top bound edge is carried out to bound edge.
The mode that adopts silk screen printing insulation compound bound edge in described step c is after completing steps a and b, makes in advance a silk screen mould consistent with titanium starting sheet top bound edge area size with frame, and silk screen mould frame is fixed on bound edge position; After brushing insulation compound, solidify titanium starting sheet, according to this method, the another side of titanium starting sheet top bound edge is carried out to bound edge.
In described step c, adopting the mode of opening dovetail-indent injection-molding edge is after completing steps a and b, goes out the dovetail-indent of degree of depth 1.5mm-2mm in the region precision work of titanium starting sheet bound edge; By the reconditioning of dovetail-indent internal surface, oil removing; Injection-molding edge in injection-molding edge machine is put into in titanium starting sheet bound edge region; After injection moulding, titanium starting sheet is put into moist closet and is solidified; According to this method, the another side in bound edge region, titanium starting sheet top is carried out to bound edge.
Beneficial effect of the present invention: the present invention is according to producing starting sheet dimensional requirement, except titanium starting sheet both sides and bottom bound edge, adopt on titanium starting sheet top and paste insulation tape or open dovetail-indent injection moulding or the mode such as artificial or silk screen printing insulation compound is carried out bound edge, the specification that can effectively control starting sheet is in optimum range; Reduce starting sheet limit portion shearing displacement, enhance productivity and product percentage of product.
Accompanying drawing explanation
Fig. 1. titanium starting sheet bound edge schematic diagram of the present invention;
Fig. 2. titanium starting sheet of the present invention top bound edge location positioning schematic diagram;
Fig. 3. titanium starting sheet of the present invention top dovetail-indent injection-molding edge schematic diagram.
Embodiment
Below in conjunction with accompanying drawing, titanium starting sheet of the present invention top Wrapping method is described further:
As shown in Figure 1, 2, bound edge position in titanium starting sheet top is determined according to the liquid level of starting sheet specification size, cathode compartment, after reserving shearing amount; The upper edge of titanium starting sheet top bound edge width is the liquid level at cathode compartment according to titanium starting sheet, conventionally on bound edge width, edge exceeds cathode compartment liquid level 20mm-50mm, and the lower edge of titanium starting sheet top bound edge width adds after surplus height is sheared on titanium starting sheet bottom bound edge height and starting sheet top and determines according to starting sheet height.The length of titanium starting sheet top bound edge and the width of titanium starting sheet are consistent.Determining after bound edge length and bound edge width, by the polishing of bound edge region, polishing, cleaning, then paste insulation tape or silk screen printing insulation compound bound edge; As shown in Figure 2, the titanium starting sheet top of carrying out dovetail-indent injection-molding edge need, after definite bound edge position and width, process dovetail-indent on titanium starting sheet two sides, by after the reconditioning of dovetail-indent internal surface, oil removing in injection-molding edge machine injection-molding edge.
embodiment 1:
Titanium starting sheet top adopts insulation tape bound edge: determine titanium starting sheet bound edge position, specific as follows: titanium starting sheet height 980mm, starting sheet height 860mm, titanium starting sheet base bound edge height 10mm, process redundancy height is 10mm, and the lower edge of top bound edge width is highly 860+10+10=880mm; Cathode compartment liquid level 950mm, on bound edge width, along exceeding cathode compartment liquid level 30mm, on bound edge width, edge is highly 950+30mm=980mm, therefore bound edge width is 980-880=100mm.The length of titanium starting sheet top bound edge and the width of titanium starting sheet are consistent.Determining after bound edge length and bound edge width.By the polishing of bound edge region, polishing, cleaning; With slide calliper rule line, insulation tape namely cuts according to titanium starting sheet top bound edge width and titanium starting sheet width the strip that length and width meet in advance according to bound edge region, titanium starting sheet top, removes insulation tape glue-line and covers, and pastes to the layout line titanium starting sheet from a direction; According to aforesaid method, the another side in bound edge region, titanium starting sheet top is carried out to bound edge.
embodiment 2:
Titanium starting sheet top adopts silk screen printing insulation compound bound edge: determine titanium starting sheet bound edge position, specific as follows: titanium starting sheet height 980mm, starting sheet height 860mm base bound edge height 10mm, process redundancy height 10mm, the end of top bound edge, is along being highly 860+10+10=880mm; Cathode compartment liquid level 930mm, on bound edge width, along exceeding cathode compartment liquid level 50mm, on bound edge, edge is highly 930+50mm=980mm, therefore bound edge width is 980-880=100mm.The length of titanium starting sheet top bound edge and the width of titanium starting sheet are consistent.Determining bound edge length and bound edge width aftertreatment bound edge region, by the polishing of bound edge region, polishing, cleaning; Make in advance one with frame with bound edge silk screen mould of the same size, with slide calliper rule line, silk screen mould frame is fixed in scribing position; With round brush brushing insulation compound, make to apply insulation compound even thickness from a direction round brush, after round brush completes titanium starting sheet keep flat aerated area solidify; According to aforesaid method, titanium starting sheet another side is carried out to bound edge.Brushing insulation compound also can, after line, adopt and manually use brush brushing.
embodiment 3:
Titanium starting sheet top adopts and opens dovetail-indent injection-molding edge: determine titanium starting sheet bound edge position, specific as follows: titanium starting sheet height 980mm, starting sheet height 860mm base bound edge height 10mm, process redundancy height 10mm, the end of top bound edge, is along being highly 860+10+10=880mm; Cathode compartment liquid level 960mm, on bound edge width, along exceeding cathode compartment liquid level 20mm, on bound edge, edge is highly 960+20mm=980mm, therefore bound edge width is 980-880=100mm.The length of titanium starting sheet top bound edge and the width of titanium starting sheet are consistent.Determining after bound edge length and bound edge width; Go out the dovetail-indent of degree of depth 1.5mm-2mm in the region precision work of titanium starting sheet bound edge; By the reconditioning of dovetail-indent internal surface, oil removing; Injection-molding edge in injection-molding edge machine is put into in titanium starting sheet bound edge region; After injection moulding, titanium starting sheet is put into moist closet and is solidified; According to aforesaid method, the another side in bound edge region, titanium starting sheet top is carried out to bound edge.
Claims (4)
1. the titanium starting sheet Wrapping method that can control starting sheet size, is characterized in that: comprise the following steps
A) determine the position of titanium starting sheet top bound edge:
Determining of titanium starting sheet top bound edge width: titanium starting sheet top bound edge wide be on bound edge width along highly and under bound edge width along the difference between height, on described bound edge width, the height on edge is determined according to exceeding cathode compartment liquid level 20-50mm, and the height that under described bound edge width, the height on edge is starting sheet adds the height of titanium starting sheet bottom bound edge and the height of starting sheet top shearing surplus;
Determining of titanium starting sheet top bound edge length: the length of titanium starting sheet top bound edge and the width of titanium starting sheet are consistent;
B) pack processing edge regions: to bound edge region polish, polishing, cleaning;
C) bound edge of titanium starting sheet: the top of titanium starting sheet is adopted and pastes insulation tape or silk screen printing insulation compound or open dovetail-indent injection moulding mode and carry out bound edge.
2. a kind of titanium starting sheet Wrapping method of controlling starting sheet size as claimed in claim 1, it is characterized in that: in described step c, adopting the mode of stickup insulation tape bound edge is after completing steps a and b, insulation tape cuts, pastes and cover titanium starting sheet top according to the size in bound edge region, titanium starting sheet top, according to this method, the another side of titanium starting sheet top bound edge is carried out to bound edge.
3. a kind of titanium starting sheet Wrapping method of controlling starting sheet size as claimed in claim 1, it is characterized in that: the mode that adopts silk screen printing insulation compound bound edge in described step c is after completing steps a and b, make in advance a silk screen mould consistent with titanium starting sheet top bound edge area size with frame, silk screen mould frame is fixed on bound edge position; After brushing insulation compound, solidify titanium starting sheet, according to this method, the another side of titanium starting sheet top bound edge is carried out to bound edge.
4. a kind of titanium starting sheet Wrapping method of controlling starting sheet size as claimed in claim 1, it is characterized in that: in described step c, adopting the mode of opening dovetail-indent injection-molding edge is after completing steps a and b, goes out the dovetail-indent of degree of depth 1.5mm-2mm in the region precision work of titanium starting sheet bound edge; By the reconditioning of dovetail-indent internal surface, oil removing; Injection-molding edge in injection-molding edge machine is put into in titanium starting sheet bound edge region; After injection moulding, titanium starting sheet is put into moist closet and is solidified; According to this method, the another side in bound edge region, titanium starting sheet top is carried out to bound edge.