CN103510389B - Spray coking wax feeling leather production method - Google Patents
Spray coking wax feeling leather production method Download PDFInfo
- Publication number
- CN103510389B CN103510389B CN201210209417.XA CN201210209417A CN103510389B CN 103510389 B CN103510389 B CN 103510389B CN 201210209417 A CN201210209417 A CN 201210209417A CN 103510389 B CN103510389 B CN 103510389B
- Authority
- CN
- China
- Prior art keywords
- minutes
- parts
- dimethyl formamide
- wet
- polyurethane
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Expired - Fee Related
Abstract
The invention discloses a spray coking wax feeling leather production method comprising the steps: uniformly mixing 5 to 10 parts of dimethyl formamide and 0.5 to 2 parts of a color paste; after mixing 100 to 120 parts of dimethyl formamide and 20 to 30 parts of wood powder for swelling, adding the above-mentioned mixture; then adding 100 parts of a polyurethane wet-process resin to mix uniformly, and defoaming; coating the above-mentioned slurry on textile fabric fibers, solidifying, squeezing water, washing with water, and drying to obtain a wet-process bass; uniformly mixing 100 parts of a polyurethane dry-process color-changing resin, 15 to 20 parts of dimethyl formamide, 15 to 20 parts of butanone, 15 to 20 parts of toluene, 0.5 to 1.0 part of an auxiliary agent and 3 to 5 parts of a toner; carrying out scrape coating of the above-mentioned slurry on release paper, after drying, cohering with the wet-process bass, and then separating from the release paper; uniformly mixing 100 parts of a polyurethane treating agent, 20 to 30 parts of butyl acetate and 5 to 10 parts of the color paste, after spraying on clothes prepared from the above-mentioned material, drying, then wrinkling, washing with water, and drying. The surface of an obtained synthetic leather layer has a coking wax feeling.
Description
Technical field
The present invention relates to a kind of artificial leather preparation method, particularly one sprays burnt wax sense leather preparation method.
Background technology
Traditional artificial leather is base cloth layer, wet method bass layer and dry method overlay coating composition, and make artificial leather entirety shrivelled, stiff, visual effect is undesirable, gives inflexible sensation, is difficult to meet and the demand of the costume design in modern times.
Summary of the invention
In order to overcome above-mentioned defect, the invention provides a kind of spraying burnt wax sense leather preparation method, this spraying burnt wax sense leather preparation method technique is simple, and the product surface produced has burnt wax sense, and colour contrast is large, and Tructure arrangement is obvious, and visual effect is strong.
The present invention in order to the technical scheme solving its technical problem and adopt is: a kind of spraying burnt wax sense leather preparation method, and concrete steps are as follows:
Step one: wet-mixing is prepared burden:
A. by 5 ~ 10kg dimethyl formamide and 0.5 ~ 2kg mill base high-speed stirred 80 ~ 100 minutes, then filter stand-by;
B. by 100 ~ 120kg dimethyl formamide and 20 ~ 30kg wood powder mix and blend 20 ~ 30 minutes, then fully swelling 30 ~ 40 minutes, then add the mixture filtered in step a and stir stand-by;
C. 100kg polyurethane wet resin is joined in the mixture that step b formed, stir 30 ~ 40 minutes, deaeration 40 ~ 50 minutes;
Step 2: wet method bass is produced:
Being coated with by the slurry that in step one, deaeration has been formed scrapes on woven fabric fiber, immersing mass percentage concentration is again solidify in the dimethylformamide in water of 18 ~ 22%, then through at least one squezzing operation, more a kind of wet method bass after carrying out washing and drying, is obtained;
Step 3: dry mixed is prepared burden:
By even for high-speed stirred after the mixing of 100kg polyurethane dry method color-change resin, 15 ~ 20kg dimethyl formamide, 15 ~ 20kg butanone, 15 ~ 20kg toluene, 0.5 ~ 1.0kg auxiliary agent and 3 ~ 5kg toner, mixing time 10-15 minute;
Step 4: dry method veneer:
Being coated with by the dry method slurry prepared in step 3 scrapes in forming dry method veneer with in the release liners of flower pattern, then by adhesive be adhered on dry method veneer under the condition of 90 ~ 110 DEG C in temperature by the wet method bass in step 2, be separated through super-dry heel release liners, obtain a kind of semi-finished product;
Step 5: finishing agent mix:
By even for high-speed stirred after the mixing of 100kg polyurethane finishing agent, 20 ~ 30kg butyl acetate and 5 ~ 10kg mill base, mixing time 10 ~ 20 minutes, filters stand-by;
Step 6: spraying:
After the semi-finished product of step 4 make clothes, with the finishing agent of spray gun spraying step 5, dry at the temperature of 50 ~ 80 DEG C after having sprayed;
Step 7: washing:
The clothes of step 6 is put in the boarding machine that 40 ~ 60 DEG C of water are housed, clear water washes 15 ~ 30 minutes, dries, be finished product at the temperature of 70 ~ 90 DEG C.
As a further improvement on the present invention, dimethyl formamide and mill base high-speed stirred 90 minutes in described step a.
As a further improvement on the present invention, the mixed liquor of 240 order nylon wires to dimethyl formamide and mill base is used to filter in described step a;
B. by 100 ~ 120kg dimethyl formamide and 20 ~ 30kg wood powder mix and blend 30 minutes, then fully swelling 35 minutes, then add the mixture filtered in step a and stir stand-by;
C. 100kg polyurethane wet resin is joined in the mixture that step b formed, stir 40 minutes, deaeration 45 minutes;
As a further improvement on the present invention, it is characterized in that: the speed of a motor vehicle of described step 2 is at 18-20 rice/min, and the speed of a motor vehicle of step 4 is at 20-25 rice/min.
The invention has the beneficial effects as follows: the present invention, by there being the spray treatment layer of burnt wax sense in dry method overlay coating surface spraying setting tool, makes synthetic leather layer surface have burnt wax sense, colour contrast is large, and Tructure arrangement is obvious, and visual effect is strong.
Detailed description of the invention
Embodiment: a kind of spraying burnt wax sense leather preparation method, concrete steps are as follows:
Step one: wet-mixing is prepared burden:
A. by 5 ~ 10kg dimethyl formamide and 0.5 ~ 2kg mill base high-speed stirred 80 ~ 100 minutes, then filter stand-by;
B. by 100 ~ 120kg dimethyl formamide and 20 ~ 30kg wood powder mix and blend 20 ~ 30 minutes, then fully swelling 30 ~ 40 minutes, then add the mixture filtered in step a and stir stand-by;
C. 100kg polyurethane wet resin is joined in the mixture that step b formed, stir 30 ~ 40 minutes, deaeration 40 ~ 50 minutes;
Step 2: wet method bass is produced:
Being coated with by the slurry that in step one, deaeration has been formed scrapes on woven fabric fiber, immersing mass percentage concentration is again solidify in the dimethylformamide in water of 18 ~ 22%, then through at least one squezzing operation, more a kind of wet method bass after carrying out washing and drying, is obtained;
Step 3: dry mixed is prepared burden:
By even for high-speed stirred after the mixing of 100kg polyurethane dry method color-change resin, 15 ~ 20kg dimethyl formamide, 15 ~ 20kg butanone, 15 ~ 20kg toluene, 0.5 ~ 1.0kg auxiliary agent and 3 ~ 5kg toner, mixing time 10-15 minute.
Step 4: dry method veneer:
Being coated with by the dry method slurry prepared in step 3 scrapes in forming dry method veneer with in the release liners of flower pattern, then by adhesive be adhered on dry method veneer under the condition of 90 ~ 110 DEG C in temperature by the wet method bass in step 2, be separated through super-dry heel release liners, obtain a kind of semi-finished product;
Step 5: finishing agent mix:
By even for high-speed stirred after the mixing of 100kg polyurethane finishing agent, 20 ~ 30kg butyl acetate and 5 ~ 10kg mill base, mixing time 10 ~ 20 minutes, filters stand-by;
Step 6: spraying:
After the semi-finished product of step 4 make clothes, with the finishing agent of spray gun spraying step 5, dry at the temperature of 50 ~ 80 DEG C after having sprayed;
Step 7: washing:
The clothes of step 6 is put in the boarding machine that 40 ~ 60 DEG C of water are housed, clear water washes 15 ~ 30 minutes, dries, be finished product at the temperature of 70 ~ 90 DEG C.
Dimethyl formamide and mill base high-speed stirred 90 minutes in described step a.
The mixed liquor of 240 order nylon wires to dimethyl formamide and mill base is used to filter in described step a;
B. by 100 ~ 120kg dimethyl formamide and 20 ~ 30kg wood powder mix and blend 30 minutes, then fully swelling 35 minutes, then add the mixture filtered in step a and stir stand-by;
C. 100kg polyurethane wet resin is joined in the mixture that step b formed, stir 40 minutes, deaeration 45 minutes;
The speed of a motor vehicle of described step 2 is at 18-20 rice/min, and the speed of a motor vehicle of step 4 is at 20-25 rice/min.
Claims (4)
1. a spraying burnt wax sense leather preparation method, is characterized in that: concrete steps are as follows:
Step one: wet-mixing is prepared burden:
A. by 5 ~ 10kg dimethyl formamide and 0.5 ~ 2kg mill base high-speed stirred 80 ~ 100 minutes, then filter stand-by;
B. by 100 ~ 120kg dimethyl formamide and 20 ~ 30kg wood powder mix and blend 20 ~ 30 minutes, then fully swelling 30 ~ 40 minutes, then add the mixture filtered in step a and stir stand-by;
C. 100kg polyurethane wet resin is joined in the mixture that step b formed, stir 30 ~ 40 minutes, deaeration 40 ~ 50 minutes;
Step 2: wet method bass is produced:
Being coated with by the slurry that in step one, deaeration has been formed scrapes on woven fabric fiber, immersing mass percentage concentration is again solidify in the dimethylformamide in water of 18 ~ 22%, then through at least one squezzing operation, more a kind of wet method bass after carrying out washing and drying, is obtained;
Step 3: dry mixed is prepared burden:
By even for high-speed stirred after the mixing of 100kg polyurethane dry method color-change resin, 15 ~ 20kg dimethyl formamide, 15 ~ 20kg butanone, 15 ~ 20kg toluene, 0.5 ~ 1.0kg auxiliary agent and 3 ~ 5kg toner, mixing time 10-15 minute;
Step 4: dry method veneer:
Being coated with by the dry method slurry prepared in step 3 scrapes in forming dry method veneer with in the release liners of flower pattern, then by adhesive by the wet method bass in step 2 in temperature is to be adhered on dry method veneer under the condition of 90 ~ 110 DEG C, through super-dry heel from
Type paper is separated, and obtains a kind of semi-finished product;
Step 5: finishing agent mix:
By even for high-speed stirred after the mixing of 100kg polyurethane finishing agent, 20 ~ 30kg butyl acetate and 5 ~ 10kg mill base, mixing time 10 ~ 20 minutes, filters stand-by;
Step 6: spraying:
After the semi-finished product of step 4 make clothes, with the finishing agent of spray gun spraying step 5, dry at the temperature of 50 ~ 80 DEG C after having sprayed;
Step 7: washing:
The clothes of step 6 is put in the boarding machine that 40 ~ 60 DEG C of water are housed, clear water washes 15 ~ 30 minutes, dries, be finished product at the temperature of 70 ~ 90 DEG C.
2. spraying according to claim 1 burnt wax sense leather preparation method, is characterized in that: dimethyl formamide and mill base high-speed stirred 90 minutes in described step a.
3. spraying according to claim 1 burnt wax sense leather preparation method, is characterized in that: use the mixed liquor of 240 order nylon wires to dimethyl formamide and mill base to filter in described step a;
B. by 100 ~ 120kg dimethyl formamide and 20 ~ 30kg wood powder mix and blend 30 minutes, then fully swelling 35 minutes, then add the mixture filtered in step a and stir stand-by;
C. 100kg polyurethane wet resin is joined in the mixture that step b formed, stir 40 minutes, deaeration 45 minutes.
4. spraying according to claim 1 burnt wax sense leather preparation method, is characterized in that: the speed of a motor vehicle of described step 2 is at 18-20 rice/min, and the speed of a motor vehicle of step 4 is at 20-25 rice/min.