CN103409084B - sealant composition, display device and detection method - Google Patents

sealant composition, display device and detection method Download PDF

Info

Publication number
CN103409084B
CN103409084B CN201310353961.6A CN201310353961A CN103409084B CN 103409084 B CN103409084 B CN 103409084B CN 201310353961 A CN201310353961 A CN 201310353961A CN 103409084 B CN103409084 B CN 103409084B
Authority
CN
China
Prior art keywords
plastic box
sealed plastic
sealant composition
fluorescent material
box layer
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Expired - Fee Related
Application number
CN201310353961.6A
Other languages
Chinese (zh)
Other versions
CN103409084A (en
Inventor
张雨
黄华
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
BOE Technology Group Co Ltd
Original Assignee
BOE Technology Group Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by BOE Technology Group Co Ltd filed Critical BOE Technology Group Co Ltd
Priority to CN201310353961.6A priority Critical patent/CN103409084B/en
Priority to PCT/CN2013/086763 priority patent/WO2015021697A1/en
Publication of CN103409084A publication Critical patent/CN103409084A/en
Application granted granted Critical
Publication of CN103409084B publication Critical patent/CN103409084B/en
Expired - Fee Related legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

The invention discloses a kind of sealant composition, except sealed plastic box also comprises fluorescent material, wherein sealed plastic box comprises: prepolymer, reactive monomer, thermal curing agents and light trigger, sealant composition also comprises dispersion agent.By adding the fluorescent material with fluorescent effect in original sealed plastic box, making the sealant composition obtained can realize the adhesive effect of original sealed plastic box, also facilitating the detection of sealed plastic box layer bonding effect by fluorescence.The invention also discloses the display device based on above-mentioned sealant composition and detection method, sealed plastic box is placed under wavelength is less than the invisible light of 400nm and irradiates, according to the sealing-in situation of the fluorescent effect determination sealed plastic box layer of sealed plastic box layer.Therefore, it is possible to easily and effectively detect the bonding effect of sealed plastic box layer, without the need to detecting under special environment, avoiding in handling process, causing panel broken, obtaining detected result effectively fast.

Description

Sealant composition, display device and detection method
Technical field
The present invention relates to technique of display field, particularly relate to sealant composition, display device and detection method.
Background technology
At LCD(LiquidCrystalDisplay, liquid-crystal display) preparation process in, the bonding effect of sealed plastic box layer directly affects the quality of the LCD of LCD post-production and processing and fabricating.In the preparation process of LCD, the effect of sealed plastic box layer is that array substrate and color membrane substrates are sticked together, playing sealing function, ensure TFT(ThinFilmTransistor, Thin Film Transistor (TFT)) liquid crystal in the middle of array substrate and color membrane substrates is by the impact of outside air.If sealed plastic box layer existing defects in coating process, the bonding effect of sealed plastic box layer can be caused not good, the liquid crystal between array substrate and color membrane substrates all can not be closed, cause liquid crystal to leak outside.
In order to realize sealed plastic box layer, there is good bonding effect, in process of production and later stage test be all a requisite operation to the detection of sealed plastic box layer, but due in the gap very little between array substrate and color membrane substrates of sealed plastic box layer, need could detect the defect whether sealed plastic box layer exists clearly under comparatively special environment.Especially in preparation process after some special processings, as irrigation crystal operation after, the detection for sealed plastic box layer will become more inconvenient.In prior art for the detection method of sealed plastic box layer be: after sealed plastic box coating solidification completes, detect under the liquid crystal panel that testing staff obtains after color membrane substrates and tft array substrate being fitted removes microscope.The inconvenience of this kind of detection method is: testing staff needs liquid crystal panel to be transported to test zone, and the process of transporting can bring inconvenience, as broken in easily caused liquid crystal panel in handling process, program routine is also particularly complicated under the microscope, and when the area of liquid crystal panel is bigger than normal, difficulty of test can be larger, operates very difficult, make troubles to detection.
Therefore, need one not need in particular circumstances, only need to operate simply and easily the method just can carried out sealed plastic box layer bonding effect and detect.
Summary of the invention
(1) technical problem that will solve
For above-mentioned defect, the technical problem to be solved in the present invention how to reduce the requirement to environment in sealed plastic box layer testing process, realizes the detection to sealed plastic box layer more easily.
(2) technical scheme
For solving the problem, the invention provides a kind of sealant composition, comprising sealed plastic box, also comprising fluorescent material, the invisible light that described fluorescent material is less than 400nm by wavelength excites and discharges luminous energy.
Further, described fluorescent material accounts for the mass percent of described sealant composition is 1% ~ 5%.
Further, described fluorescent material is ultraviolet excitation fluorescent material.
Further, described sealed plastic box comprises: prepolymer, reactive monomer, thermal curing agents and light trigger.
Further, described sealant composition also comprises dispersion agent.
Further, described dispersion agent accounts for the mass percent of described sealant composition is 0% ~ 5%.
Further, the mass ratio of fluorescent material and described dispersion agent described in described sealant composition is 1:1.
Further, described dispersion agent is ethanol.
For solving the problem, present invention also offers a kind of display device, described display device comprises the sealed plastic box layer adopting above-mentioned sealant composition to be formed.
For solving the problem, present invention also offers a kind of detection method of the bonding effect for above-mentioned sealed plastic box layer, described method comprises:
Step C1, the described sealed plastic box utilizing described sealant composition to be formed is placed under wavelength is less than the invisible light of 400nm and irradiates;
Step C2, judge the sealing-in situation of described sealed plastic box layer according to the fluorescent effect of sealed plastic box layer each several part.
(3) beneficial effect
The invention provides a kind of sealant composition, except sealed plastic box also comprises fluorescent material, wherein sealed plastic box comprises: prepolymer, reactive monomer, thermal curing agents and light trigger.Also dispersion agent is comprised in sealant composition.By adding the fluorescent material with fluorescent effect in original sealed plastic box, making the sealant composition obtained can realize the adhesive effect of original sealed plastic box, fluorescent effect can also be utilized to facilitate the detection of sealed plastic box bonding effect.By adding fluorescent material or directly add fluorescent material in the raw materials of sealed plastic box in sealed plastic box, make the sealant composition obtained not only have the sealing function of sealed plastic box, also there is fluorescent effect.
Present invention also offers the detection method of display device and the sealed plastic box layer bonding effect comprising the sealed plastic box layer utilizing above-mentioned sealant composition to be formed, in sealed plastic box layer testing process can by wavelength be less than 400nm invisible light irradiate just can detect the bonding effect of sealed plastic box layer, and utilize microscope to detect without the need to being transported in special environment by whole display device, avoid in handling process, causing display device broken, detected result can be obtained effectively rapidly.
Accompanying drawing explanation
Fig. 1 is preparation method's flow chart of steps of a kind of sealant composition in the embodiment of the present invention two;
Fig. 2 is the flow chart of steps of scheme one in the embodiment of the present invention two;
Fig. 3 is the flow chart of steps of scheme two in the embodiment of the present invention two;
Fig. 4 is the flow chart of steps of scheme three in the embodiment of the present invention two;
Fig. 5 is a kind of structural profile schematic diagram comprising the display panels of sealed plastic box layer in the embodiment of the present invention three;
Fig. 6 is a kind of vertical view comprising the display panels of sealed plastic box layer in the embodiment of the present invention three;
Fig. 7 is a kind of flow chart of steps comprising the bonding effect detection method of sealed plastic box layer in the display panels of sealed plastic box layer in the embodiment of the present invention four.
Embodiment
Below in conjunction with drawings and Examples, the specific embodiment of the present invention is described in further detail.Following examples for illustration of the present invention, but are not used for limiting the scope of the invention.
Embodiment one
Present embodiments provide a kind of sealant composition, comprise sealed plastic box, also comprise fluorescent material.
In order to ensure the fluorescent effect of sealant composition, do not affect its degree of adhesion again, the ratio of fluorescent material is generally in the scope of 1% ~ 5% simultaneously.
Wherein sealed plastic box comprises: prepolymer, reactive monomer, thermal curing agents and light trigger.
Add fluorescent material in the composition in the present embodiment, can also add dispersion agent, preferably, the mass percent of dispersion agent is 0 ~ 5% simultaneously.Dispersant adsorption also significantly can reduce interfacial free energy in liquid-solid interface, and pressed powder is dispersed in liquid or melt uniformly.Dispersion agent is as a kind of interfacial agent simultaneously in molecule with lipophilicity and wetting ability two kinds of opposite nature, can homogeneous dispersion those be difficult to be dissolved in the inorganic of liquid or organic solid particulate, also can prevent sedimentation and the cohesion of solid particulate simultaneously, contribute to forming the medicament needed for stable suspension.Dispersion agent without any effect for the fluorescent effect of sealed plastic box, is not the necessary component of sealant composition simultaneously, can not adds, namely 0 in aforementioned proportion scope.
Preferably, what select in the present embodiment be dispersion agent is ethanol.This dispersion agent also can be that other anyly can play to fluorescent material the material that dissemination can not impact other composition in sealed plastic box again simultaneously in other embodiments.
The present embodiment adds dispersion agent in sealant composition, and the mass ratio adding fluorescent material and dispersion agent is preferably 1:1.The effect of dispersion agent is dispersed in sealed plastic box by the fluorescent material of powdery, if it is not obvious to add too paucidisperse effect, if add too much, again can other requires impact on viscosity of sealant composition etc., when therefore adding dispersion agent, preferably according to being that 1:1 adds with fluorescent material mass ratio.
In the present embodiment, fluorescent material can not be excited under visible light illumination, cannot produce fluorescent effect, but can be excited be less than the irradiation of the invisible light (UV-light in such as the present embodiment) of 400nm at wavelength under and discharge luminous energy, produces fluorescent effect.Why select the irradiation being less than the invisible light of 400nm at wavelength herein, because the light source of use when display device works is visible ray, if this visible ray can excitation fluorescent material, so can because the fluorescent effect of sealed plastic box layer affect display effect when display device shows.
For ultraviolet excitation fluorescent material in the present embodiment, sealant composition can realize being excited under the irradiation of UV-light and storing luminous energy, detects the bonding effect of sealed plastic box to facilitate.
Embodiment two
Provide a kind of preparation method of sealant composition in the present embodiment, steps flow chart as shown in Figure 1, specifically comprises the following steps:
Step S1: the sealant composition by adding fluorescent material preparation with fluorescent effect.
Step S2: defoaming treatment is carried out to the sealant composition with fluorescent effect, obtains sealant composition.
Aforesaid method by adding fluorescent material in sealed plastic box, and make the sealant composition obtained have fluorescent effect, the sealant composition utilizing the method to obtain not only has the sealing function of sealed plastic box, also has fluorescent effect.
Step S1 preparation is had to the sealant composition of fluorescent effect, present embodiments provide one preferably scheme one, step S1 specifically comprises:
Step S11: thaw to sealed plastic box, obtains the sealed plastic box of thawing.
Step S12: fluorescent material is joined in the sealed plastic box after thawing, obtain the sealant composition with fluorescent effect.
Sealed plastic box is first thawed by step S11 ~ S12, adds the fluorescent material that weight percent is 1% in sealed plastic box.The thawing time of usual sealed plastic box is 50 minutes to 100 minutes, preferably 60 minutes.After thawing, carry out the Homogeneous phase mixing of fluorescent material and sealed plastic box, should avoid polluting in mixing process, can not stir with ferrous material.
Step S2 processes the sealant composition with fluorescent effect that above-mentioned steps obtains, and obtains sealant composition.Concrete process is defoaming treatment, or is called deaeration process, and above-mentioned sealant composition is carried out deaeration process in deaerating agent, and the time of deaeration process is generally 20 minutes to 40 minutes, preferably 30 minutes.Sealant composition is obtained after deaeration process; this kind of sealant composition not only has good bonding effect, and the liquid crystal realizing filling between array substrate and color membrane substrates carries out closed protective, also has the effect of fluorescence; easily identify under UV-irradiation, convenient detection.
Employing scheme one realizes the steps flow chart of the preparation method of sealant composition as shown in Figure 2.
Fluorescent material directly joins in the sealed plastic box after thawing by above-mentioned this programme one, can also be first in fluorescent material, add dispersion agent, mix with the sealed plastic box of thawing, therefore the present embodiment additionally provides best scheme two, and wherein step S1 specifically comprises again:
Step S11 ': thaw to sealed plastic box, obtains the sealed plastic box of thawing;
Step S12 ': add dispersion agent in the ratio of 1:1 and mix in fluorescent material, then mixing with the sealed plastic box after thawing, obtaining the sealant composition with fluorescent effect.
Also will thaw to sealed plastic box in step S11 ' in the program, the method for thawing and requirement are same as scheme one.Be to add dispersion agent in proportion in fluorescent material with the difference of scheme one, the ratio of fluorescent material and dispersion agent is generally 1:1, can improve the fluorescent effect of fluorescent material by adding dispersion agent in the composition.
In like manner, step S2 carries out defoaming treatment to the sealant composition with fluorescent effect and is also same as scheme one, does not repeat them here.Employing scheme two realizes the steps flow chart of the preparation method of sealant composition as shown in Figure 3.
Scheme one and scheme two are all first thaw to sealed plastic box, fluorescent material is added in sealed plastic box after thawing, the present embodiment additionally provides scheme three, just fluorescent material is added in the making processes of sealed plastic box, fluorescent material is joined in the raw materials of sealed plastic box, obtain the sealant composition with fluorescent effect.
Wherein the raw materials of sealed plastic box is prepolymer or reactive monomer.Although the thermal curing agents also comprised in the raw materials of sealed plastic box except prepolymer and reactive monomer and light trigger, but be all the auxiliary material in sealed plastic box preparation process by thermal curing agents and light trigger, therefore fluorescent material will be added in main raw material prepolymer or reactive monomer.
Scheme three step S2 carries out defoaming treatment to the sealant composition with fluorescent effect and is also same as scheme one, does not repeat them here.Employing scheme three realizes the steps flow chart of the preparation method of sealant composition as shown in Figure 4.
It should be noted that; such scheme one, two and three is all the preferred forms provided for the present embodiment; protection scope of the present invention is not only scheme one, two and three, and other replacement carried out on the basis of such scheme all should drop within protection scope of the present invention.
The preparation method of the sealant composition that the present embodiment provides, first preparation has the sealant composition of fluorescent effect, directly can add fluorescent material by the sealed plastic box of thawing, or join in the sealed plastic box after thawing after first fluorescent material dispersion agent being mixed again, or directly fluorescent material can also be joined in the raw materials of sealed plastic box and obtain sealant composition, again defoaming treatment is carried out to sealant composition, finally obtain the sealant composition of not bubbles.By adding fluorescent material in sealed plastic box after thawing or directly adding fluorescent material in the raw materials of sealed plastic box, the sealant composition obtained is made to have fluorescent effect, the sealant composition utilizing the method to obtain not only has the sealing function of sealed plastic box, also has fluorescent effect.
Embodiment three
Provide a kind of display device in the present embodiment, comprise the sealed plastic box layer formed by sealant composition described in above-described embodiment one.
Preferably, display device in the present embodiment is for display panels, wherein the diagrammatic cross-section of display panels as shown in Figure 5, and wherein 8 is color membrane substrates, and 9 is array substrate, 5 is sealed plastic box layer, and the liquid crystal panel shown in Fig. 5 also comprises polaroid 1, glass substrate 2, black matrix (BM) 3, oriented layer 4, liquid crystal 6 and chock insulator matter 7.
As shown in Figure 6, wherein 2 is glass substrate to the vertical view of the display panels that the present embodiment provides, and 5 is sealed plastic box layer, and 3 is black matrix B M, and 10 is display space.
Wherein said display device can also be: any product or parts with Presentation Function such as Electronic Paper, oled panel, mobile phone, panel computer, televisor, indicating meter, notebook computer, DPF, navigating instrument.
Embodiment four
Provide the detection method of the bonding effect of the sealed plastic box layer in a kind of display device provided for above-described embodiment three in the present embodiment, as shown in Figure 7, described method comprises steps flow chart:
Step C1, the described sealed plastic box utilizing described sealant composition to be formed is placed under wavelength is less than the invisible light of 400nm and irradiates;
Step C2, judge the sealing-in situation of described sealed plastic box layer according to the fluorescent effect of sealed plastic box layer each several part.
Above-mentioned detection method is normally carried out in darkroom, and darkroom refers to the room of shading device, or the space of dark; Its Main Function is the convenient fluorescent effect detecting sealed plastic box layer.
The present embodiment, for display panels, specifically comprises the following steps:
Step D1, the color membrane substrates utilizing sealant composition to bond and array substrate be placed under wavelength is less than the invisible light of 400nm and irradiate.
Whether step D2, intact according to closing of the fluorescent effect determination sealed plastic box layer of sealed plastic box layer, sealed plastic box layer is solidify to form by sealant composition.
According to the preparation method of sealant composition in the sealant composition of above-described embodiment one and embodiment two, the sealant composition obtained is carried out defoaming treatment, obtain sealant composition, again it is coated on substrate surface surrounding by glue spreading apparatus, instillation liquid crystal, carry out box, then solidify to form sealed plastic box layer.
Fluorescent effect described in step d 2 comprises luminous intensity and luminous continuity, wherein luminous intensity represents whether the thickness of sealed plastic box layer meets the requirements, if the less thick of sealed plastic box layer, luminous intensity is dimmed, undesirable, otherwise luminous intensity is constant, meet the requirements; Luminous continuity represents whether sealed plastic box layer is continuous coating, if luminous continuity is unchanged, sealed plastic box layer is coating continuously, otherwise sealed plastic box layer is not continuous coating.If the thickness low LCL of sealed plastic box will cause liquid crystal to leak outside, luminous intensity is exactly the main reference judging sealed plastic box thickness.
Determine that whether intact closing of sealed plastic box layer specifically comprise in step d 2: judge whether closing of sealed plastic box layer be intact according to luminous intensity, if the luminous intensity of sealed plastic box layer is dimmed, not sealed plastic box layer closed not intact, otherwise sealed plastic box layer is closed intact; Or
Judge whether closing of sealed plastic box layer be intact according to luminous continuity, if the luminous continuity of sealed plastic box layer changes, closing of sealed plastic box layer is not intact, otherwise sealed plastic box layer is closed intact.Sealed plastic box continuous print is detected whether be coated with complete detection to the sealed plastic box layer of liquid crystal cell surrounding exactly.
Below the present embodiment for add in sealed plastic box mass percent be 1% fluorescent material obtain sealant composition and be described, sealed plastic box wherein in the present embodiment can be the one in HC1850, HC1840, XN-5A, S-WB73-1 and S-UR96-2, because fluorescent material is inorganics, do not react with the organism in sealed plastic box, so the interpolation of fluorescent material is applicable to all sealed plastic boxs, the embodiment of the present invention is only described for HC1850.
There is provided sealant composition and application thereof for above-described embodiment, below enumerate specific examples and be described:
Example 1
With reference to the scheme one in embodiment two, first 60 minutes thawing is carried out to sealed plastic box, then by mass percent be 1% ultraviolet excited fluorescence powder join in the sealed plastic box after thawing, just obtain the sealant composition comprising 1% fluorescent material.Then the sealant composition obtained is carried out to the defoaming treatment of 30 minutes, obtain the sealant composition of not bubbles.
Then the sealant composition obtained is coated on substrate surface surrounding, carry out after instillation liquid crystal array substrate and color membrane substrates position to box, sealant composition is cured, array substrate and color membrane substrates are glued together by sealant composition, form sealed plastic box layer in liquid crystal cell surrounding simultaneously.
Finally, in darkroom, by the fluorescent effect of sealed plastic box layer, bonding effect is detected.Irradiate under above-mentioned liquid crystal panel being placed in invisible light (as UV-light), observe the fluorescent effect of sealed plastic box layer.Due to sealed plastic box layer comprises burst of ultraviolel should light powder, can be excited under the irradiation of UV-light.Just can determine whether closing of sealed plastic box layer be intact according to the fluorescent effect of sealed plastic box layer, avoid trouble that the liquid crystal panel made moves up everywhere in sealed plastic box testing process, save labour turnover, therefore according to the fluorescent effect of sealed plastic box layer, bonding effect is detected, convenient and simple.
Wherein the fluorescent effect of sealed plastic box layer comprises luminous intensity and luminous continuity, can judge whether the thickness that sealed plastic box layer is coated with meets the requirements by detecting luminous intensity, can judge whether sealed plastic box layer is continuous uniform coating by detecting luminous continuity.
Example 2
Be with the difference of example 1, this example with the addition of the dispersion agent that mass percent is 1%, the scheme two of preparation method's reference embodiment two of concrete sealant composition, concrete: by mass percent be 1% ultraviolet excitation fluorescent material and mass percent be 1% dispersant even, the mixture obtained is joined in the sealed plastic box of thawing again, the sealant composition comprising 1% fluorescent material and 1% dispersion agent can be obtained.Other steps are all identical with example 1.
Example 3
This example is that the mass ratio first according to 1:1 in ultraviolet excitation fluorescent material adds dispersion agent equally, but it is different from the adding proportion of scheme two, the i.e. fluorescent material of 5% and the dispersion agent of 5%, still be prepared according to the preparation flow of such scheme two, obtain the sealant composition comprising 5% fluorescent material and 5% dispersion agent.Other steps are all identical with example 2.
The preparation method of the sealant composition that above-mentioned three kinds of examples adopt is exemplary, also can adopt the additive method in embodiment two or additive method of the prior art.
Comparative example
This comparative example is do not add fluorescent material in sealed plastic box after thawing with the difference of example 1, and other steps are all identical with example 1.
Below the fluorescent effect of the sealed plastic box layer that above-mentioned three examples and comparative example obtain and bonding effect are contrasted, as shown in table 1.
The detected result of table 1 sealed plastic box layer
According to table 1 Comparative result, add dispersion agent and can improve fluorescent effect, brightness increases, make detection convenient, but if the decline of bonding effect will be caused during the large percentage added according to dispersion agent in example three and ultraviolet excited fluorescence powder, therefore, preferably, the adding proportion of fluorescent material (the ultraviolet excited fluorescence powder namely in the present embodiment) will control below 5%.
Use the sealant composition prepared of the present embodiment to prepare display panels, after it is to box, the detection method of the bonding effect adopting the present embodiment to provide, by experiment, detects its panel and to split the bonding effect of situation, checking sealed plastic box layer.First the color membrane substrates utilizing sealant composition to bond and array substrate are put and irradiate under ultraviolet light, according to luminous intensity and luminous continuity whether sealed plastic box layer closed again and intactly to judge, if the luminous intensity of sealed plastic box layer is dimmed, closing of sealed plastic box layer is not intact, otherwise sealed plastic box layer is closed intact; If the luminous continuity of sealed plastic box layer changes, closing of sealed plastic box layer is not intact, otherwise sealed plastic box layer is closed intact.This detection method just can detect the bonding effect of sealed plastic box layer by means of only fluorescent effect, and utilize microscope to detect without the need to being transported in special environment by whole liquid crystal panel, avoid in handling process, causing panel broken, detected result can be obtained effectively rapidly.Due to fast easy to detect, the efficiency of detection therefore can also be improved.
Above embodiment is only for illustration of the present invention; and be not limitation of the present invention; the those of ordinary skill of relevant technical field; without departing from the spirit and scope of the present invention; can also make a variety of changes and modification; therefore all equivalent technical schemes also belong to category of the present invention, and scope of patent protection of the present invention should be defined by the claims.

Claims (3)

1. a sealant composition, comprises sealed plastic box, it is characterized in that, also comprises fluorescent material, and the invisible light that described fluorescent material is less than 400nm by wavelength excites and discharges luminous energy;
Described sealed plastic box comprises: prepolymer, reactive monomer, thermal curing agents and light trigger;
The mass percent that described fluorescent material accounts for described sealant composition is 1% ~ 5%;
Described fluorescent material is ultraviolet excitation fluorescent material;
Described sealant composition also comprises dispersion agent;
The mass ratio of fluorescent material and described dispersion agent described in described sealant composition is 1:1;
Described dispersion agent is ethanol.
2. a display device, is characterized in that, described display device comprises the sealed plastic box layer adopting sealant composition formation described in claim 1.
3. for a detection method for the bonding effect of the sealed plastic box layer of display device according to claim 2, it is characterized in that, described method comprises:
Step C1, the described sealed plastic box utilizing described sealant composition to be formed is placed under wavelength is less than the invisible light of 400nm and irradiates;
Step C2, judge the sealing-in situation of described sealed plastic box layer according to the fluorescent effect of sealed plastic box layer each several part.
CN201310353961.6A 2013-08-14 2013-08-14 sealant composition, display device and detection method Expired - Fee Related CN103409084B (en)