CN103289266B - 一种水溶性塑料包装袋及其制备方法 - Google Patents

一种水溶性塑料包装袋及其制备方法 Download PDF

Info

Publication number
CN103289266B
CN103289266B CN201310252581.3A CN201310252581A CN103289266B CN 103289266 B CN103289266 B CN 103289266B CN 201310252581 A CN201310252581 A CN 201310252581A CN 103289266 B CN103289266 B CN 103289266B
Authority
CN
China
Prior art keywords
parts
water
packing bag
plastic packing
soluble plastic
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Expired - Fee Related
Application number
CN201310252581.3A
Other languages
English (en)
Other versions
CN103289266A (zh
Inventor
张卫
蒋学功
张美英
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Suzhou New District Jiahe Plastics Co Ltd
Original Assignee
Suzhou New District Jiahe Plastics Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Suzhou New District Jiahe Plastics Co Ltd filed Critical Suzhou New District Jiahe Plastics Co Ltd
Priority to CN201310252581.3A priority Critical patent/CN103289266B/zh
Publication of CN103289266A publication Critical patent/CN103289266A/zh
Application granted granted Critical
Publication of CN103289266B publication Critical patent/CN103289266B/zh
Expired - Fee Related legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

本发明公开了一种水溶性塑料包装袋及其制备方法,包括以下重量份计的组分:聚乙烯醇30-40份、淀粉20-30份、增塑剂10-20份、氧化锌6-7份、松焦油1-2份、丙烯菊酯10-12份、双硫化苄4-10份、水杨酸2-20份、表面活性剂1-10份、防粘剂5-20份、渗透剂6-13份、pH调节剂2-10份、防腐剂5-15份。本发明的水溶性包装袋可降解环保安全,在土壤中迅速降解,不会影响周围的环境;耐热性强;对被包装的产品无危害,延长产品的寿命周期。

Description

一种水溶性塑料包装袋及其制备方法
技术领域
本发明涉及塑胶领域,尤其涉及一种水溶性塑料包装袋及其制备方法。
背景技术
塑料包装袋作为一种包装材料,被广泛应用于各种产品的包装,如农药、化肥、染料、水处理剂、混凝土增强材料及园艺护理的化学试剂等;使用安全方便,避免使用者直接接触被包装物,可用于对人体有害物品的包装。但是塑料包装袋不易降解,严重污染环境;有些地方虽然对塑料包装袋进行处理,但是降解处理的产物同样或多或少会对环境造成危害,从而形成二次污染。聚乙烯塑料包装制品。属一次性包装用品,价格低廉,在日常生活中被广泛应用。由于基本上没有回收利用价值,回收率极低,因其质轻和难以降解的特性造成随风 漂移,污染土地和水面,占我国已形成的白色垃圾中的主要组成部分。目前,我国已明令禁止超薄膜塑料袋的生产、销售和使用。本发明提供一种水溶性塑料包装袋,以解决塑料包装袋造成的废弃物污染问题。
发明内容
本发明提供了一种水溶性塑料包装袋及其制备方法,可降解且降解产物对环境无污染,环保安全。
本发明采用以下技术方案:
一种水溶性塑料包装袋,包括以下重量份计的组分:
聚乙烯醇30-40份、淀粉20-30份、增塑剂10-20份、氧化锌6-7份、松焦油1-2份、丙烯菊酯10-12份、双硫化苄4-10份、水杨酸2-20份、表面活性剂1-10份、防粘剂5-20份、渗透剂6-13份、pH 调节剂2-10份、防腐剂5-15份。
聚乙烯醇具有很好的生物降解性,对环境的污染为零,PVA 在较高浓度(1%~12%)下对土壤物理性状具有积极作用;浓度为万分之一的PVA 也有显著的形成土壤水稳性团粒的能力,浓度为千分之一的PVA 已具有极显著形成土壤水稳性团粒结构,使土壤水分散失量减少,可抑止土壤酸化,减少土壤钾流失,使土壤的化学、物理性状得到改善。
为了提高其水溶性,聚乙烯醇的醇解度优选66%~78%,因为聚乙烯醇的溶解性随其醇解度的高低而有很大差别,醇解度小于66%,由于憎水的乙酰基含量增大,水溶性下降到醇解度在50%以下,聚乙烯醇即不再溶于水。
PVA 是聚乙酸乙烯酯经不同程度醇解后的产物,分子中有大量羟基(-OH)和酰基(-OCCH3),这些基团的存在,使得这些物质的分子和分子链键间产生强烈的结合作用,形成很大的结合力,导致它们难在室温和低温下溶于水,意外的发现加入上述比例的淀粉后,淀粉能够提供能量能破坏这种结合力,同时中和淀粉包装袋发硬发脆的缺陷,又融入了PVA包装袋较好的强度性能和柔顺性。
聚乙烯醇本身具有吸湿性,一般的增塑剂会增加包装袋的吸湿性,为了避免这种反应,本发明最好选择邻苯二甲酸二丁酯作为增塑剂。
为了进一步改善包装袋的水溶性,表面活性剂最好选择脂肪酸钠。
渗透剂优选脂肪醇或聚氧乙烯醚,目的是增加分子间的距离或调节阻隔物质,在保证这些水溶性键的完好存在条件下,破坏或降低分子间的作用,让水分子进入这些物质分子间顺利结合而易溶于水。
防粘剂优选玻璃微珠、硅藻土、滑石或碳酸钙中的一种。
防腐剂优选亚硝酸盐或二氧化硫,目的是在形成包装袋后性能优良,不受环境影响和不影响环境。
pH调节剂优选碳酸钠或碳酸钾,目的是控制和调节不同溶解温度要求。
上述包装袋的制备方法包括以下步骤:先将原料混合均匀制成水溶性胶,再流延涂布到镜面不锈钢带上,进入干燥室干燥至水分含量为5-8%,成膜后从钢带上剥离,切边收卷。
本发明的水溶性包装袋在水中可以完全溶解,不产生有害物质,可降解环保安全,在土壤中迅速降解,不会影响周围的环境;耐热性强;其拉伸强度在120MPa,断裂拉伸率仅2%左右;挥发物含量在2.5mg/100ml以下,对被包装的产品无危害,延长产品的寿命周期;在180℃高温条件下,热稳定时间可以达到40分钟以上,不易损坏。
具体实施方式
下面结合具体实施例对本发明作进一步详细介绍。
实施例1
    一种水溶性塑料包装袋,包括以下重量份计的组分:醇解度为66%的聚乙烯醇30份、淀粉20份、邻苯二甲酸二丁酯10份、氧化锌6份、松焦油1份、丙烯菊酯10份、双硫化苄4份、水杨酸2份、脂肪酸钠1份、玻璃微珠5份、脂肪醇6份、碳酸钠2份、亚硝酸盐5份。
    上述包装袋的制备方法包括以下步骤:先将原料混合均匀制成水溶性胶,再流延涂布到镜面不锈钢带上,进入干燥室干燥至水分含量为5%,成膜后从钢带上剥离,切边收卷。
实施例2
    一种水溶性塑料包装袋,包括以下重量份计的组分:醇解度为78%的聚乙烯醇40份、淀粉30份、邻苯二甲酸二丁酯20份、氧化锌7份、松焦油2份、丙烯菊酯12份、双硫化苄10份、水杨酸20份、脂肪酸钠10份、硅藻土20份、聚氧乙烯醚13份、碳酸钾10份、亚二氧化硫15份。
    上述包装袋的制备方法包括以下步骤:先将原料混合均匀制成水溶性胶,再流延涂布到镜面不锈钢带上,进入干燥室干燥至水分含量为8%,成膜后从钢带上剥离,切边收卷。
实施例3
    一种水溶性塑料包装袋,包括以下重量份计的组分:醇解度为68%的聚乙烯醇35份、淀粉25份、邻苯二甲酸二丁酯15份、氧化锌6.5份、松焦油1.5份、丙烯菊酯11份、双硫化苄8份、水杨酸13份、脂肪酸钠5份、碳酸钙15份、聚氧乙烯醚10份、碳酸钠7份、亚硝酸盐8份。
    上述包装袋的制备方法包括以下步骤:先将原料混合均匀制成水溶性胶,再流延涂布到镜面不锈钢带上,进入干燥室干燥至水分含量为6%,成膜后从钢带上剥离,切边收卷。
下面通过试验测试实施例1、2、3制得的产品的性能:
项目 测试方法 实施例1 实施例2 实施例3
拉伸强度MPa ASTM D-638 110.5 120.8 116.4
断裂拉伸率% ASTM D-638 2.1 2.3 1.9
溶解性(30±5℃水中) -- 完全溶解 完全溶解 完全溶解
降解率% -- 98 93 96
挥发物含量(mg/100ml) -- 2.3 2.1 2.5
热稳定时间(180℃,分) ASTM D-746 40 45 49

Claims (8)

1.一种水溶性塑料包装袋,其特征在于包括以下重量份计的组分:聚乙烯醇30-40份、淀粉20-30份、增塑剂10-20份、氧化锌6-7份、松焦油1-2份、丙烯菊酯10-12份、双硫化苄4-10份、水杨酸2-20份、表面活性剂1-10份、防粘剂5-20份、渗透剂6-13份、pH 调节剂2-10份、防腐剂5-15份;渗透剂是脂肪醇或聚氧乙烯醚。
2.根据权利要求1所述的水溶性塑料包装袋,其特征在于:聚乙烯醇的醇解度为66%~78%。
3.根据权利要求1所述的水溶性塑料包装袋,其特征在于:增塑剂是邻苯二甲酸二丁酯。
4.根据权利要求1所述的水溶性塑料包装袋,其特征在于:表面活性剂是脂肪酸钠。
5.根据权利要求1所述的水溶性塑料包装袋,其特征在于:防粘剂是玻璃微珠、硅藻土、滑石或碳酸钙中的一种。
6.根据权利要求1所述的水溶性塑料包装袋,其特征在于:防腐剂是亚硝酸盐或二氧化硫。
7.根据权利要求1所述的水溶性塑料包装袋,其特征在于:pH调节剂是碳酸钠或碳酸钾。
8.基于权利要求1所述的水溶性塑料包装袋的制备方法,其特征在于包括以下步骤:先将原料混合均匀制成水溶性胶,再流延涂布到镜面不锈钢带上,进入干燥室干燥至水分含量为5-8%,成膜后从钢带上剥离,切边收卷。
CN201310252581.3A 2013-06-24 2013-06-24 一种水溶性塑料包装袋及其制备方法 Expired - Fee Related CN103289266B (zh)