CN103045772A CN2012105671893A CN201210567189A CN103045772A CN 103045772 A CN103045772 A CN 103045772A CN 2012105671893 A CN2012105671893 A CN 2012105671893A CN 201210567189 A CN201210567189 A CN 201210567189A CN 103045772 A CN103045772 A CN 103045772A
Authority
CN
China
Prior art keywords
leather
cladding
treatment
remains
processing
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CN2012105671893A
Other languages
Chinese (zh)
Inventor
吴炳坤
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
SUZHOU MINGJIN TEXTILE CO Ltd
Original Assignee
SUZHOU MINGJIN TEXTILE CO Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by SUZHOU MINGJIN TEXTILE CO Ltd filed Critical SUZHOU MINGJIN TEXTILE CO Ltd
Priority to CN2012105671893A priority Critical patent/CN103045772A/en
Publication of CN103045772A publication Critical patent/CN103045772A/en
Pending legal-status Critical Current

Links

Landscapes

  • Treatment And Processing Of Natural Fur Or Leather (AREA)

Abstract

The invention discloses a processing technology for manufacturing leather by waste leather. The method comprises the processing steps that (1), the smashed waste leather is subjected to tanning treatment; (2), the tanned leather is subjected to dyeing treatment; (3), the dyed leather is subjected to fat liquoring treatment; and (4), the leather subjected to the fat liquoring treatment is subjected to retanning treatment. With the adoption of the scheme disclosed by the invention, the processing technology for manufacturing the leather by the waste leather is simple in operation and high in finished product rate, and the manufactured leather is low in cost and good in wear-resisting performance.

Description

A kind of complete processing of utilizing waste and old cladding to make leather
Technical field
The present invention relates to the leather preparation field, particularly relate to a kind of complete processing of utilizing waste and old cladding to make leather.
Background technology
The Chinese leather industry is optimized structure through adjusting, and has begun to take shape in the whole nation that a collection of division of labor based on specialization is clear and definite, characteristic outstanding, the pulling local economy has been played leather production characteristic zone and the specialized market of very important effect.As everyone knows, the daily necessitiess such as fur clothing, leather shoes, corium sofa belong to easy loss product, and it updates than very fast, throw away a lot of waste and old claddings because of natural renewal, wear and tear every year, not only cause the pollution of environment, also cause the waste of material.And behind the scrap leather and the pulverizing of corium tankage with various animals, the leather that allotment industrial chemicals processing and fabricating forms, its surface processing technique is the same with the skin of having a shave, the embossed leather of corium, the hide edge is more neat, utilization ratio is high, low price, but the skin body is generally thicker, intensity is relatively poor, setting process product and the par belts such as a suitable for making par briefcase, pull bar bag, club cover.
Summary of the invention
The technical problem that the present invention mainly solves provides a kind of waste and old cladding that utilizes simple to operate and makes the complete processing of leather, and the leather quality of making is good, wear resisting property is good, can be used for making the daily necessitiess such as sofa, case and bag.
For solving the problems of the technologies described above, the technical scheme that the present invention adopts is: a kind of complete processing of utilizing waste and old cladding to make leather is provided, comprises following processing step:
(1) the waste and old cladding after will pulverizing carries out tanning and processes,
(2) processing of dyeing of the cladding after tanning is processed,
The cladding that (3) will dye after processing carries out the stuffing processing,
(4) cladding after the stuffing processing being carried out retanning processes.
In a preferred embodiment of the present invention, described tanning treatment solution PH remains on 3.5-4.5, and described tanning treatment temp remains on the 25-50 degree, and the described tanning treatment time is 10-15 hour.
In a preferred embodiment of the present invention, described dyeing treatment solution PH remains on 4.5-5.5, and described dyeing treatment temp remains on the 45-65 degree, and the described dyeing treatment time is 2-5 hour.
In a preferred embodiment of the present invention, described stuffing treatment solution PH remains on 4-6, and described stuffing treatment temp remains on the 40-70 degree, and the described stuffing treatment time is 1-2 hour.
In a preferred embodiment of the present invention, described retanning treatment solution PH remains on 4-6, and described retanning treatment temp remains on the 25-55 degree, and the described retanning treatment time is 1-2 hour.
The invention has the beneficial effects as follows: the present invention utilizes waste and old cladding to make that the leather cost that the complete processing of leather is simple to operate, yield rate is high, be made is low, wear resisting property good.
Embodiment
The below is described in detail preferred embodiment of the present invention, thereby so that advantages and features of the invention can be easier to be it will be appreciated by those skilled in the art that protection scope of the present invention is made more explicit defining.
A kind of complete processing of utilizing waste and old cladding to make leather comprises following processing step:
(1) the waste and old cladding after will pulverizing carries out tanning and processes, and utilizes trivalent chromic ion that the collagen group of hide fiber is coupled together, and gives leather plentiful feel, increase the intensity of the anti-stretch-draw of leather, anti tear, select vegetable tanning agent, the leather that the filling personality is good, hardness large, make is abundant
(2) processings of dyeing of the cladding after tanning is processed gives cladding certain color, and key is to improve the combination rate of dyestuff and hide fiber, improves the intensity of dyestuff and hide fiber combination, water-fastness by force,
The cladding that (3) will dye after processing carries out the stuffing processing, allows cladding absorb an amount of stuffing material, prevents stiff plate of cladding, cracking,
(4) cladding after stuffing is processed carries out retanning and processes, and can replenish the tanning effect, improves content of tannin, makes physical properties of leather more even, and that improves leather goes out the sanction rate.
In addition, described tanning treatment solution PH remains on about 4, and described tanning treatment temp remains on 35 degree, and the described tanning treatment time is 13 hours.
In addition, described dyeing treatment solution PH remains on about 5, and described dyeing treatment temp remains on 50 degree, and the described dyeing treatment time is 3 hours.
In addition, described stuffing treatment solution PH remains on about 5, and described stuffing treatment temp remains on 60 degree, and the described stuffing treatment time is 1.5 hours.
In addition, described retanning treatment solution PH remains on about 5.5, and described retanning treatment temp remains on 40 degree, and the described retanning treatment time is 2 hours.
The leather that the complete processing that the present invention utilizes waste and old cladding to make leather processes, can be used for making sofa, case and bag etc. is not too high daily necessities to the leather quality requirement, its Costco Wholesale is low, wear resisting property good, water-fastness, arrange well.
Be different from prior art, the present invention utilizes waste and old cladding to make that the leather cost that the complete processing of leather is simple to operate, yield rate is high, be made is low, wear resisting property good.
The above only is embodiments of the invention; be not so limit claim of the present invention; every equivalent structure or equivalent flow process conversion that utilizes specification sheets of the present invention to do, or directly or indirectly be used in other relevant technical fields, all in like manner be included in the scope of patent protection of the present invention.

Claims (5)

1. a complete processing of utilizing waste and old cladding to make leather is characterized in that, comprises following processing step:
(1) the waste and old cladding after will pulverizing carries out tanning and processes,
(2) processing of dyeing of the cladding after tanning is processed,
The cladding that (3) will dye after processing carries out the stuffing processing,
(4) cladding after the stuffing processing being carried out retanning processes.
2. the complete processing of utilizing waste and old cladding to make leather according to claim 1 is characterized in that, described tanning treatment solution PH remains on 3.5-4.5, and described tanning treatment temp remains on the 25-50 degree, and the described tanning treatment time is 10-15 hour.
3. the complete processing of utilizing waste and old cladding to make leather according to claim 1 is characterized in that, described dyeing treatment solution PH remains on 4.5-5.5, and described dyeing treatment temp remains on the 45-65 degree, and the described dyeing treatment time is 2-5 hour.
4. the complete processing of utilizing waste and old cladding to make leather according to claim 1 is characterized in that, described stuffing treatment solution PH remains on 4-6, and described stuffing treatment temp remains on the 40-70 degree, and the described stuffing treatment time is 1-2 hour.
5. the complete processing of utilizing waste and old cladding to make leather according to claim 1 is characterized in that, described retanning treatment solution PH remains on 4-6, and described retanning treatment temp remains on the 25-55 degree, and the described retanning treatment time is 1-2 hour.
CN2012105671893A 2012-12-25 2012-12-25 Processing technology for manufacturing leather by waste leather Pending CN103045772A (en)

Priority Applications (1)

Application Number Priority Date Filing Date Title
CN2012105671893A CN103045772A (en) 2012-12-25 2012-12-25 Processing technology for manufacturing leather by waste leather

Applications Claiming Priority (1)

Application Number Priority Date Filing Date Title
CN2012105671893A CN103045772A (en) 2012-12-25 2012-12-25 Processing technology for manufacturing leather by waste leather

Publications (1)

Publication Number Publication Date
CN103045772A true CN103045772A (en) 2013-04-17

Family

ID=48058631

Family Applications (1)

Application Number Title Priority Date Filing Date
CN2012105671893A Pending CN103045772A (en) 2012-12-25 2012-12-25 Processing technology for manufacturing leather by waste leather

Country Status (1)

Country Link
CN (1) CN103045772A (en)

Cited By (2)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
CN108085436A (en) * 2016-11-19 2018-05-29 江苏天成超纤革业有限公司 The method of comprehensive utilization and device of a kind of leather castoff
CN113999944A (en) * 2021-11-02 2022-02-01 江苏金太阳家用纺织品有限公司 Preparation method of fabric containing antibacterial cow leather

Citations (5)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JPH04285700A (en) * 1991-03-15 1992-10-09 Tetsuo Imai Production of leather board
KR100833277B1 (en) * 2007-07-05 2008-05-28 주식회사 해성아이다 Process for processing natural leather without chromium and tanning composition
TW200948971A (en) * 2008-05-19 2009-12-01 Liu Hsu Method of preparing protein filler for leather by using animal hair
RU2405043C1 (en) * 2009-09-18 2010-11-27 Лесник Дмитрий Иванович Method of processing and hardening skins of birds for production of fur out wear
CN101914637A (en) * 2010-08-18 2010-12-15 辉县市明德皮业有限公司 Chrome-tanned, water-dyed and polished leather manufacturing method

Patent Citations (5)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JPH04285700A (en) * 1991-03-15 1992-10-09 Tetsuo Imai Production of leather board
KR100833277B1 (en) * 2007-07-05 2008-05-28 주식회사 해성아이다 Process for processing natural leather without chromium and tanning composition
TW200948971A (en) * 2008-05-19 2009-12-01 Liu Hsu Method of preparing protein filler for leather by using animal hair
RU2405043C1 (en) * 2009-09-18 2010-11-27 Лесник Дмитрий Иванович Method of processing and hardening skins of birds for production of fur out wear
CN101914637A (en) * 2010-08-18 2010-12-15 辉县市明德皮业有限公司 Chrome-tanned, water-dyed and polished leather manufacturing method

Cited By (2)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
CN108085436A (en) * 2016-11-19 2018-05-29 江苏天成超纤革业有限公司 The method of comprehensive utilization and device of a kind of leather castoff
CN113999944A (en) * 2021-11-02 2022-02-01 江苏金太阳家用纺织品有限公司 Preparation method of fabric containing antibacterial cow leather

Similar Documents

Publication Publication Date Title
CN103060488B (en) Environment-friendly type crust leather production method
CN101463397B (en) Method for manufacturing chromium-free tanning environment protection pigskin shoes
CN104789715B (en) One kind is salt-free to exempt from pickling short route less chrome tannage method
CN106521048B (en) The fur leather integrated dyeing of lamb
CN104962667A (en) Quick producing process for pure vegetable tanning cattle leather
CN104818354A (en) Processing technology for chrome-free tanning leather
Rathinamoorthy et al. Bacterial cellulose—a sustainable alternative material for footwear and leather products
CN105925735B (en) One kind is salt-free to exempt from pickling short route bating method without chrome
CN101812551A (en) Technology for imitating mink fur by using rabbit fur
CN103045772A (en) Processing technology for manufacturing leather by waste leather
CN104673943A (en) Method for manufacturing environment-friendly ecological tanned lamb skin
EP2862944B1 (en) Ecological tanning and dyeing process and product obtained
CN101381782A (en) Method for tanning ultrathin sheepskin garment leather using non-chromium metal composite tanning agents
CN102943138A (en) Manufacturing method of highly tear resistant ultrathin boot leather
CN108950100B (en) Production process of original thick environment-friendly shrunk-pattern cattle leather
CN102312023B (en) Secondary recycling method of pigskin chrome-free combination tannage waste liquid
CN102888434A (en) Process of extracting collagen from waste chrome leather scraps
CN104087688A (en) Modified rice dialdehyde starch retanning filler for leather and preparation method of filler
CN105543422B (en) Make the method for book-binding leather and its book-binding leather of making using rabbit leather
CN103555866A (en) Ecological automobile leather manufacturing method by adopting novel enzyme unhairing
CN103103296B (en) The method of tear strength of leather is improved without deashing and softening
CN102409114B (en) Damp effect technology for pretreatment before combination tannage of metal salts and tannin extract
CN112391857A (en) Dyeing process for improving leveling property of shorn cashmere fine leather
CN112575129B (en) Environment-friendly rabbit fur leather integrated manufacturing method
CN115595387B (en) Efficient leather production method based on aldehyde tanning agent

Legal Events

Date Code Title Description
C06 Publication
PB01 Publication
C10 Entry into substantive examination
SE01 Entry into force of request for substantive examination
C02 Deemed withdrawal of patent application after publication (patent law 2001)
WD01 Invention patent application deemed withdrawn after publication

Application publication date: 20130417