CN102926215A - Cotton-polyester blended fabric pretreatment method - Google Patents

Cotton-polyester blended fabric pretreatment method Download PDF

Info

Publication number
CN102926215A
CN102926215A CN2012104941908A CN201210494190A CN102926215A CN 102926215 A CN102926215 A CN 102926215A CN 2012104941908 A CN2012104941908 A CN 2012104941908A CN 201210494190 A CN201210494190 A CN 201210494190A CN 102926215 A CN102926215 A CN 102926215A
Authority
CN
China
Prior art keywords
destarch
enzyme
premium
desizing
polyester cotton
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CN2012104941908A
Other languages
Chinese (zh)
Inventor
王力民
罗维新
楚云荣
李春光
吕建品
姚永旺
刘宁宁
刘跃霞
张炳营
王绪山
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
HUAFANG CO Ltd
Original Assignee
HUAFANG CO Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by HUAFANG CO Ltd filed Critical HUAFANG CO Ltd
Priority to CN2012104941908A priority Critical patent/CN102926215A/en
Publication of CN102926215A publication Critical patent/CN102926215A/en
Pending legal-status Critical Current

Abstract

The invention relates to the blended fabric dyeing and finishing technology, and particularly relates to a cotton-polyester blended fabric pretreatment method. The invention aims at providing a pretreatment method which can solve the problems of thinness and stiffness of the cotton-polyester blended fabric after conventional dyeing and finishing and improves the fullness, fluffiness and woolen feel. The cotton-polyester blended fabric pretreatment method comprises the processes of desizing, bleaching, setting, mercerizing and the like; the desizing is performed by an enzyme desizing cold batch technology; and in the desizing process, a desizing enzyme and a penetrant are added. According to the invention, through a great quantity of technological tests and process point optimization of the long car pretreatment process, the fiber is sufficiently puffed, the thickness, woolen feel, desizing rate, capillary effect and whiteness of the fabric are improved, and the pretreatment cost is lowered.

Description

The polyester cotton pre-treating method
Technical field
The present invention relates to the BLENDED FABRIC dyeing and printing process, be specially a kind of polyester cotton pre-treating method.
Background technology
Clothes processing variation, feel style no longer are parked on the interface such as soft, sliding, stiffening, glossy, require abundant, fluffy also getting more and more.Appearance is thin, stiff, shortage is plentiful, fluffy, the style of the feel of wool and polyester-cotton fabric is understood after the long vehicle common process is processed.
Summary of the invention
The object of the invention is to provide a kind of pre-treating method, can solve occur after the conventional dyeing and finishing of polyester cotton is processed thin, stiff, increases its plentiful, fluffy, feel of wool.
Concrete technical scheme of the present invention is: a kind of polyester cotton pre-treating method, comprise the operations such as destarch, bleaching, typing and mercerising, and the enzyme desizing cold batching process is adopted in described destarch, in the destarch operation, adds destarch enzyme and bleeding agent.
In the described destarch operation, every premium on currency adds destarch enzyme 2000L 19-21g, penetrant t A-1 2.5-3.5g; 45-50 ℃ of material hopper temperature, even running 8 circles of A cabinet frame/minute, bank up 10 hours time; Padding machine pressure should be controlled at 0.15-0.17Mpa behind each rinsing bowl.
In the described bleaching process, every premium on currency adds 100% hydrogen peroxide 10-11 g, complex enzyme Ai Tuoer element YC-669B 9-11 g; 93-95 ℃ of L-box temperature, steam pressure 0.06-0.08Mpa banks up 35 minutes time.
Described setting process condition is 210 ℃ ± 1 ℃ of temperature, 30 seconds-35 seconds time.
Every premium on currency adds NaOH 210-220g in the described mercerizing process.
As selection process, in the described destarch operation, every premium on currency adds destarch enzyme 2000L 20g, penetrant t A-1 3g; 45-50 ℃ of material hopper temperature, even running 8 circles of A cabinet frame/minute, bank up 10 hours time; In the described bleaching process, every premium on currency adds 100% hydrogen peroxide 10.5g, complex enzyme Ai Tuoer element YC-669B 10 g; 93-95 ℃ of L-box temperature, steam pressure 0.06-0.08Mpa banks up 35 minutes time.
Beneficial effect of the present invention is: the present invention is at a large amount of engineer testings of long vehicle pretreatment procedure process, Optimization Technology point, fiber is fully expanded, increased thickness, the velvet of fabric, destarch rate, capillary effect, whiteness, reduced simultaneously the pre-treatment cost, this technique is a greatly innovation of field of printing and dyeing.
The specific embodiment
Embodiment 1:
Polyester cotton is carried out pre-treatment, and its technique comprises following operation:
Destarch: every premium on currency adds destarch enzyme 2000L 20g, penetrant t A-1 3g; 45-50 ℃ of material hopper temperature, even running 8 circles of A cabinet frame/minute, bank up 10 hours time.
Bleaching: every premium on currency adds 100% hydrogen peroxide 10.5g, complex enzyme Ai Tuoer element YC-669B 10 g; 93-95 ℃ of L-box temperature, steam pressure 0.06-0.08Mpa banks up 35 minutes time.
Typing: process conditions are 210 ℃ ± 1 ℃ of temperature, 30 seconds-35 seconds time.
Mercerising: every premium on currency adds NaOH 210-220g.
Padding machine pressure should be controlled at 0.15-0.17Mpa behind each rinsing bowl.Can not press cloth too solidly, so that it is plentiful, fluffy.
Above operation touches the mark: desizing grade 8-9 level, capillary effect: 4.8cm/min.
Embodiment 2:
In the destarch operation, every premium on currency adds destarch enzyme 2000L 19g, penetrant t A-1 3.5g;
In the bleaching process, every premium on currency adds 100% hydrogen peroxide 11g, complex enzyme Ai Tuoer element YC-669B 9 g.
All the other are with embodiment 1.
Embodiment 3:
In the destarch operation, every premium on currency adds destarch enzyme 2000L 21g, penetrant t A-1 2.5g;
In the bleaching process, every premium on currency adds 100% hydrogen peroxide 10g, complex enzyme Ai Tuoer element YC-669B 11 g.
All the other are with embodiment 1.
Applicant's statement, the present invention illustrates each technological process of detailed process equipment of the present invention by above-described embodiment, but the present invention is not limited to above-mentioned detailed process equipment and process flow process, does not mean that namely the present invention must rely on above-mentioned detailed process equipment and process flow process and could implement.The person of ordinary skill in the field should be understood that any improvement in the present invention, and the interpolation of machine auxiliary element, the selection of concrete mode etc. are replaced in the equivalence of each raw material of product of the present invention, all drops within protection scope of the present invention and the open scope.

Claims (6)

1. a polyester cotton pre-treating method comprises the operations such as destarch, bleaching, typing and mercerising, it is characterized in that, the enzyme desizing cold batching process is adopted in described destarch, in the destarch operation, adds destarch enzyme and bleeding agent.
2. polyester cotton pre-treating method according to claim 1 is characterized in that, in the described destarch operation, every premium on currency adds destarch enzyme 2000L 19-21g, penetrant t A-1 2.5-3.5g; 45-50 ℃ of material hopper temperature, even running 8 circles of A cabinet frame/minute, bank up 10 hours time; Padding machine pressure should be controlled at 0.15-0.17Mpa behind each rinsing bowl.
3. polyester cotton pre-treating method according to claim 2 is characterized in that, in the described bleaching process, every premium on currency adds 100% hydrogen peroxide 10-11 g, complex enzyme Ai Tuoer element YC-669B 9-11 g; 93-95 ℃ of L-box temperature, steam pressure 0.06-0.08Mpa banks up 35 minutes time.
4. according to claim 1 and 2 or 3 described polyester cotton pre-treating methods, it is characterized in that, described setting process condition is 210 ℃ ± 1 ℃ of temperature, 30 seconds-35 seconds time.
5. according to claim 1 and 2 or 3 described polyester cotton pre-treating methods, it is characterized in that, every premium on currency adds NaOH 210-220g in the described mercerizing process.
6. according to claim 1 and 2 or 3 described polyester cotton pre-treating methods, it is characterized in that, in the described destarch operation, every premium on currency adds destarch enzyme 2000L 20g, penetrant t A-1 3g; 45-50 ℃ of material hopper temperature, even running 8 circles of A cabinet frame/minute, bank up 10 hours time; In the described bleaching process, every premium on currency adds 100% hydrogen peroxide 10.5g, complex enzyme Ai Tuoer element YC-669B 10 g; 93-95 ℃ of L-box temperature, steam pressure 0.06-0.08Mpa banks up 35 minutes time.
CN2012104941908A 2012-11-28 2012-11-28 Cotton-polyester blended fabric pretreatment method Pending CN102926215A (en)