CN102863231B - 凹凸棒火山碎屑岩粘土质熟料粉 - Google Patents

凹凸棒火山碎屑岩粘土质熟料粉 Download PDF

Info

Publication number
CN102863231B
CN102863231B CN2012103731334A CN201210373133A CN102863231B CN 102863231 B CN102863231 B CN 102863231B CN 2012103731334 A CN2012103731334 A CN 2012103731334A CN 201210373133 A CN201210373133 A CN 201210373133A CN 102863231 B CN102863231 B CN 102863231B
Authority
CN
China
Prior art keywords
chamotte powder
clayey
attapulgite
rock
volcanoclastic rock
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Expired - Fee Related
Application number
CN2012103731334A
Other languages
English (en)
Other versions
CN102863231A (zh
Inventor
许庆华
李学东
许盛英
袁长兵
蒋文兰
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Rugao Fan Chuan Trading Co Ltd
Original Assignee
许庆华
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by 许庆华 filed Critical 许庆华
Priority to CN2012103731334A priority Critical patent/CN102863231B/zh
Publication of CN102863231A publication Critical patent/CN102863231A/zh
Application granted granted Critical
Publication of CN102863231B publication Critical patent/CN102863231B/zh
Expired - Fee Related legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

本发明公开了一种凹凸棒火山碎屑岩粘土质熟料粉,其技术方案的要点是,凹凸棒火山碎屑岩粘土质熟料粉由凹凸棒石粘土尾矿、火山碎屑岩混合物、铝土矿尾矿、煤矸石和蒙脱石尾矿组成。凹凸棒火山碎屑岩粘土质熟料粉的生产方法:将凹凸棒火山碎屑岩粘土质熟料粉的配料搅拌均匀进行粉碎、浸泡、挤压、焙烧、磨粉后包装为凹凸棒火山碎屑岩粘土质熟料粉的成品。凹凸棒火山碎屑岩粘土质熟料粉具有耐火性能好和高温下不软化的特点。本发明的配料中大量采用各种废弃物,不仅有利于提高资源利用率,变废为宝,还能减少占用土地,保护和净化环境,节省能源,降低生产成本,提高经济效益,凹凸棒火山碎屑岩粘土质熟料粉适用于砌筑耐火工程。

Description

凹凸棒火山碎屑岩粘土质熟料粉
技术领域
本发明涉及耐火材料,具体涉及一种凹凸棒火山碎屑岩粘土质熟料粉。
背景技术
耐火材料主要是以粘土、铝矾土、硅石、菱镁矿、白云石等天然矿石为原料经加工后制造而成的。
我国矿产资源80%为共伴生矿,大量有价值资源存留于尾矿之中,尾矿堆存需要占用大量土地。很多尾矿库超期或超负荷使用,甚至违规操作,使尾矿库存在极大的安全隐患,对周边地区的人民财产和生命安全造成严重威胁。
凹凸棒石粘土除含凹凸棒石外,常含有蒙脱石、高岭石、水云母、海泡石、石英、蛋白石及碳酸盐等矿物。
与凹凸棒石粘土矿共生的还有火山碎屑岩,火山碎屑岩大多在凹凸棒石粘土矿的上层,有的凹凸棒石粘土矿区上层的火山碎屑岩矿层厚度高达数十米,在凹凸棒石粘土在开采过程中,凹凸棒石粘土矿区上层的火山碎屑岩作为废弃物抛弃,据实地考察,每开采1吨凹凸棒石粘土,产生的火山碎屑岩有30吨以上,按年产15万吨的产量计算,产生的火山碎屑岩高达450万吨,多年来都没有能得到利用,整个矿区到处是重新堆积的火山碎屑岩混合物,造成严重的资源浪费和经济损失。
煤矸石弃置不用,占用大片土地,煤矸石中的硫化物逸出或浸出会污染大气、农田和水体,矸石山还会自燃发生火灾,或在雨季崩塌,淤塞河流造成灾害。
发明内容
本发明的目的是克服现有技术中不足之处,提供一种凹凸棒火山碎屑岩粘土质熟料粉。
凹凸棒火山碎屑岩粘土质熟料粉由凹凸棒石粘土尾矿、火山碎屑岩混合物、铝土矿尾矿、煤矸石和蒙脱石尾矿组成。
凹凸棒火山碎屑岩粘土质熟料粉的生产方法:将凹凸棒火山碎屑岩粘土质熟料粉的配料搅拌均匀进行粉碎、浸泡、挤压、焙烧、磨粉后包装为凹凸棒火山碎屑岩粘土质熟料粉的成品。
凹凸棒石粘土是一种层链状结构的含水富镁铝硅酸盐粘土矿物,凹凸棒石粘土土质细腻,吸水性强,湿时具粘性和可塑性,有利于原料之间的粘结。
凹凸棒石粘土在开采过程中会混杂有一定量的碎石和泥土,作为一种尾矿抛弃,造成大量的资源浪费,本发明选用凹凸棒石粘土尾矿的颗粒细度≤2.0毫米。
火山碎屑岩是介于岩浆熔岩和沉积岩之间的过渡类型的岩石,其中50%以上的成分是由火山碎屑流喷出的物质组成,这些火山碎屑主要是火山上早期凝固的熔岩、通道周围在火山喷发时被炸裂的岩石形成的。火山碎屑岩混合物包括岩屑、晶屑、玻璃质屑、浆屑、火山块(直径大于100毫米)、火山砾(直径大于2毫米)和火山灰(直径小于2毫米),火山碎屑岩主要化学成分是二氧化硅和氧化铝,具有较好的耐火性能和增加凹凸棒火山碎屑岩粘土质熟料粉的强度,本发明选用火山碎屑岩混合物的颗粒细度≤5.0毫米。
铝土矿尾矿中氧化铝的含量≥38%,有利于提高凹凸棒火山碎屑岩粘土质熟料粉的强度和耐火性能,本发明选用铝土矿尾矿的颗粒细度≤2.0毫米。
煤矸石是采煤过程和洗煤过程中排放的固体废物,具有低发热值,含碳20~30%,使用煤矸石可以节约部分煤炭,增加氧化铝的含量,本发明选用煤矸石的颗粒细度≤3.0毫米。
本发明选用的蒙脱石尾矿大多分布在凹凸棒石粘土矿的下层,很难进行独立开采,但是蒙脱石尾矿质地较硬,适合生产耐火骨料,本发明选用蒙脱石尾矿的颗粒细度≤2.0毫米。
本发明通过下述技术方案予以实现:
1、凹凸棒火山碎屑岩粘土质熟料粉的配料按重量百分比由下列组分组成:凹凸棒石粘土尾矿5~25%、火山碎屑岩混合物10~40%、铝土矿尾矿5~40%、煤矸石2~20%和蒙脱石尾矿2~20%;
所述凹凸棒火山碎屑岩粘土质熟料粉的生产方法:⑴将凹凸棒火山碎屑岩粘土质熟料粉的配料加入已经运行的双卧轴强制式搅拌机中搅拌,搅拌均匀后输入粉碎机中粉碎为凹凸棒火山碎屑岩粘土质熟料粉的混合物,凹凸棒火山碎屑岩粘土质熟料粉混合物的颗粒细度≤0.2毫米;⑵将凹凸棒火山碎屑岩粘土质熟料粉混合物输入浸泡池中加水浸泡,浸泡时间控制在24~72小时;⑶将浸泡后的凹凸棒火山碎屑岩粘土质熟料粉混合物输入对辊挤压机中挤压为片状物,片状物的厚度≤3.0毫米;⑷将凹凸棒火山碎屑岩粘土质熟料粉的片状物输入回转式焙烧窑中焙烧,焙烧温度控制在650~950℃;⑸将冷却后的凹凸棒火山碎屑岩粘土质熟料粉的片状物输入磨粉机中加工为粉状物,粉状物的颗粒细度≤0.074毫米,包装为凹凸棒火山碎屑岩粘土质熟料粉的成品;
所述将凹凸棒火山碎屑岩粘土质熟料粉混合物输入浸泡池中加水浸泡时的配料,按重量百分比由下列组分组成:凹凸棒火山碎屑岩粘土质熟料粉混合物60~80%和水20~40%。
凹凸棒火山碎屑岩粘土质熟料粉具有耐火性能好和高温下不软化的特点。
凹凸棒火山碎屑岩粘土质熟料粉的配料中大量采用各种废弃物,不仅有利于提高资源利用率,变废为宝,还能减少占用土地,保护和净化环境,节省能源,降低生产成本,提高经济效益。
凹凸棒火山碎屑岩粘土质熟料粉适用于砌筑耐火工程。
具体实施方式
下面结合实施例对本发明作进一步的描述: 
凹凸棒火山碎屑岩粘土质熟料粉的配料按重量百分比由下列组分组成:凹凸棒石粘土尾矿16%、火山碎屑岩混合物32%、铝土矿尾矿28%、煤矸石16%和蒙脱石尾矿8%;
所述凹凸棒火山碎屑岩粘土质熟料粉的生产方法:⑴将凹凸棒火山碎屑岩粘土质熟料粉的配料加入已经运行的双卧轴强制式搅拌机中搅拌,搅拌均匀后输入粉碎机中粉碎为凹凸棒火山碎屑岩粘土质熟料粉的混合物,凹凸棒火山碎屑岩粘土质熟料粉混合物的颗粒细度≤0.2毫米;⑵将凹凸棒火山碎屑岩粘土质熟料粉混合物输入浸泡池中加水浸泡,浸泡时间控制在36小时;⑶将浸泡后的凹凸棒火山碎屑岩粘土质熟料粉混合物输入对辊挤压机中挤压为片状物,片状物的厚度≤3.0毫米;⑷将凹凸棒火山碎屑岩粘土质熟料粉的片状物输入回转式焙烧窑中焙烧,焙烧温度控制在800~900℃;⑸将冷却后的凹凸棒火山碎屑岩粘土质熟料粉的片状物输入磨粉机中加工为粉状物,粉状物的颗粒细度≤0.074毫米,包装为凹凸棒火山碎屑岩粘土质熟料粉的成品;
所述将凹凸棒火山碎屑岩粘土质熟料粉混合物输入浸泡池中加水浸泡时的配料,按重量百分比由下列组分组成:凹凸棒火山碎屑岩粘土质熟料粉混合物68%和水32%。

Claims (1)

1.一种凹凸棒火山碎屑岩粘土质熟料粉,其特征在于,凹凸棒火山碎屑岩粘土质熟料粉的配料按重量百分比由下列组分组成:凹凸棒石粘土尾矿5~25%、火山碎屑岩混合物10~40%、铝土矿尾矿5~40%、煤矸石2~20%和蒙脱石尾矿2~20%;
所述凹凸棒火山碎屑岩粘土质熟料粉的生产方法:⑴将凹凸棒火山碎屑岩粘土质熟料粉的配料加入已经运行的双卧轴强制式搅拌机中搅拌,搅拌均匀后输入粉碎机中粉碎为凹凸棒火山碎屑岩粘土质熟料粉的混合物,凹凸棒火山碎屑岩粘土质熟料粉混合物的颗粒细度≤0.2毫米;⑵将凹凸棒火山碎屑岩粘土质熟料粉混合物输入浸泡池中加水浸泡,浸泡时间控制在24~72小时;⑶将浸泡后的凹凸棒火山碎屑岩粘土质熟料粉混合物输入对辊挤压机中挤压为片状物,片状物的厚度≤3.0毫米;⑷将凹凸棒火山碎屑岩粘土质熟料粉的片状物输入回转式焙烧窑中焙烧,焙烧温度控制在650~950℃;⑸将冷却后的凹凸棒火山碎屑岩粘土质熟料粉的片状物输入磨粉机中加工为粉状物,粉状物的颗粒细度≤0.074毫米,包装为凹凸棒火山碎屑岩粘土质熟料粉的成品;
所述将凹凸棒火山碎屑岩粘土质熟料粉混合物输入浸泡池中加水浸泡时的配料,按重量百分比由下列组分组成:凹凸棒火山碎屑岩粘土质熟料粉混合物60~80%和水20~40%。
CN2012103731334A 2012-09-30 2012-09-30 凹凸棒火山碎屑岩粘土质熟料粉 Expired - Fee Related CN102863231B (zh)