CN102198456A - Magnesium alloy profile extrusion die cleaning device and method - Google Patents

Magnesium alloy profile extrusion die cleaning device and method Download PDF

Info

Publication number
CN102198456A
CN102198456A CN2011100728867A CN201110072886A CN102198456A CN 102198456 A CN102198456 A CN 102198456A CN 2011100728867 A CN2011100728867 A CN 2011100728867A CN 201110072886 A CN201110072886 A CN 201110072886A CN 102198456 A CN102198456 A CN 102198456A
Authority
CN
China
Prior art keywords
magnesium alloy
die
right half
half module
drift
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CN2011100728867A
Other languages
Chinese (zh)
Inventor
蔡乐勤
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
RUI'AN LEQIN AVIATION PARTS CO Ltd
Original Assignee
RUI'AN LEQIN AVIATION PARTS CO Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by RUI'AN LEQIN AVIATION PARTS CO Ltd filed Critical RUI'AN LEQIN AVIATION PARTS CO Ltd
Priority to CN2011100728867A priority Critical patent/CN102198456A/en
Publication of CN102198456A publication Critical patent/CN102198456A/en
Pending legal-status Critical Current

Abstract

The invention discloses a magnesium alloy profile extrusion die cleaning device and method. The method comprises the following steps of: separating a left half die from a right half die of a magnesium alloy profile extrusion die; placing a sleeve-shaped right half die cushion on a platform of a press, and placing the right half die which is filled with magnesium alloy in a tap hole on an extrusion die cushion; assembling an extruding punch on a slide block of the press, adapting the lower end of the right half die to the appearance of the tap hole one the right half die; and driving the extruding punch to move downward by the slide block of the press, extruding the residual magnesium alloy from the tap hole of the right half die, and leading the residual magnesium alloy in a tube cavity of the extrusion die cushion. By adopting the method for cleaning the magnesium alloy profile extrusion die, the extrusion punch is driven to extrude the magnesium alloy left in the right half die through the press; and compared with the conventional method for cleaning the extrusion die of the magnesium alloy profile, a section of the aluminum bar is saved, and alkali consumed when the die is boiled and energy consumed in heating alkaline water can be saved simultaneously.

Description

The cleaning plant of magnesium alloy profiles extrusion die and method
Technical field
The present invention relates to the cleaning of magnesium alloy profiles extrusion die, be specifically related to the cleaning plant and the method for magnesium alloy profiles extrusion die.
Background technology
Magnesium alloy profiles has advantages such as light weight, good rigidly, corrosion resistance and dimensionally stable, is widely used in fields such as Aero-Space, automobile, mobile phone, notebook computer.
Magnesium alloy profiles is by the mould extrusion modling, and in use, the fineness of die surface can very fast reduction, and this just needs in time residual magnesium alloy in the cleaning mould, polishes to repair a die, so that guarantee the fineness of section bar.
The cleaning work of magnesium alloy profiles extrusion die is a great problem in the domestic and international magnesium alloy profiles extrusion process of production always, the cleaning of magnesium alloy profiles extrusion die is different with aluminium alloy extruded mould, since aluminium alloy promptly can and acid reaction, again can and alkali reaction, but mould discord alkali reaction, therefore, aluminium alloy extruded mould can boil with buck, after treating that aluminium in the mould and alkali reaction consume, mould is opened repaired a die again.But, because magnesium not with alkali reaction, so the magnesium alloy extrusion die can not repair a die with said method.If clean with acid, then mould also can be corroded.As seen, the cleaning work of magnesium alloy profiles extrusion die is a great problem in the production process always.
The structural representation of magnesium alloy profiles extrusion die as shown in Figure 1 and Figure 2, comprise the left and right half module 10,20 that assembly forms, right half module 20 is provided with a plurality of tap holes 50, squeeze out magnesium alloy profiles 40 by left and right half module 10,20, but, after extruding is finished, can fill up residual magnesium alloy 30 in the tap hole 50 on the right half module 20.Method commonly used at present is with a joint aluminium bar magnesium alloy remaining in the mould 30 to be ejected behind extrusion magnesium alloy, and then with the method cleaning mould of cleaning aluminium alloy, can waste one section aluminium bar like this, and the aluminium that boils in the mould consumes alkali that carries out chemical reaction with it and the energy that heats buck again, in addition, some aluminium can be residual when ejecting magnesium alloy, these residual aluminium can infiltrate when next extrusion magnesium alloy in the magnesium alloy and to change its composition and performance is scrapped the part section bar, therefore must manage to remove, produce for extruding and bring additional workload.That is to say, the method for cleaning of existing magnesium alloy profiles extrusion die, not only loaded down with trivial details but also increased processing cost.
Summary of the invention
Technical problem to be solved by this invention is to solve cleaning magnesium alloy profiles extrusion die, and is not only loaded down with trivial details but also increased the problem of processing cost.
In order to solve the problems of the technologies described above, the technical solution adopted in the present invention provides a kind of cleaning plant of magnesium alloy profiles extrusion die, comprise forcing press, extrude drift and extrude die-cushion, described upper end of extruding drift is provided with and is used for and the fixing interface of the slide block of described forcing press, the shape of the tap hole on lower end and the described right half module is suitable, the described die-cushion of extruding is the cover tubular, extrude on the platform that die-cushion places described forcing press, described right half module place described extrude on the die-cushion and under the described suppressing action of extruding drift, the residual magnesium alloy of described right half module tap hole extruded drop in the described tube chamber of extruding die-cushion.
In the cleaning plant of above-mentioned magnesium alloy profiles extrusion die, also comprise die sinking drift and die sinking cushion block, the upper end of described die sinking drift is equipped with and is used for and the fixing interface of the slide block of described forcing press, the lower end is provided with and the wedge-shaped part that is used to open described left half module and right half module, the upper surface of described die sinking cushion block is provided with and the suitable arc groove of the outer circumference surface of described magnesium alloy profiles extrusion die, described die sinking cushion block places on the platform of described forcing press, and described magnesium alloy profiles extrusion die places on the described die sinking cushion block and open a described left side under the suppressing action of the wedge-shaped part of described die sinking drift, right half module.
The present invention also provides a kind of method for cleaning of magnesium alloy profiles extrusion die, may further comprise the steps:
A10, will process magnesium alloy profiles the magnesium alloy profiles extrusion die left and right half module separately;
A20, on the platform of forcing press, put the right half module pad of cover tubular, the right half module that fills up magnesium alloy in the tap hole placed extrude on the die-cushion, tap hole be positioned at described extrude die-cushion directly over;
A30, install on the slide block of forcing press and extrude drift, the profile of extruding the lower end of drift and the tap hole on the right half module is suitable;
A40, the slide block of forcing press is driven extrude drift and move down, magnesium alloy residual in the tap hole with right half module is extruded, and drops in the described tube chamber of extruding die-cushion.
In said method, steps A 10 may further comprise the steps:
A101, on the platform of forcing press, place the die sinking cushion block, the magnesium alloy profiles extrusion die is placed the die sinking cushion block;
A102, the die sinking drift is installed on the slide block of forcing press, the wedge-shaped part of die sinking drift lower end is aimed at the interface place of the left and right half module of magnesium alloy profiles extrusion die;
A103, make the slide block of forcing press drive the die sinking drift to move down, open the left and right half module of magnesium alloy profiles extrusion die.
The method for cleaning of magnesium alloy profiles extrusion die provided by the invention, extrude by the magnesium alloy that forcing press driving extruding drift will remain in the right half module, compare with the method for the cleaning extrusion die of existing magnesium alloy profiles, saved one section aluminium bar on the one hand, saved the alkali that consumes when boiling mould simultaneously and heated the energy that buck consumes.
Description of drawings
Fig. 1 is the structural representation of magnesium alloy profiles extrusion die;
Fig. 2 is the structural representation of right half module;
Fig. 3 opens the schematic diagram of left and right half module for the cleaning plant of magnesium alloy profiles extrusion die;
Fig. 4 extrudes the schematic diagram of residual magnesium alloy in the right half module for the cleaning plant of magnesium alloy profiles extrusion die.
The specific embodiment
Below in conjunction with accompanying drawing the present invention is made detailed explanation.
As shown in Figure 3, Figure 4, the cleaning plant of magnesium alloy profiles extrusion die provided by the invention comprises forcing press 1, die sinking drift 3 and extrudes drift 6 and die sinking cushion block 4 and extrude die-cushion 7.
Die sinking drift 3 and the upper end of extruding drift 6 are equipped with and are used for and the fixing interface of the slide block 2 of forcing press 1, and the lower end of die sinking drift 3 is provided with the wedge-shaped part that is used to open left and right half module, and the shape of extruding the lower end of drift 6 and the tap hole on the right half module 20 is suitable.
The upper surface of die sinking cushion block 4 is provided with and the suitable arc groove of the outer circumference surface of magnesium alloy profiles extrusion die, die sinking cushion block 4 places on the platform 5 of forcing press 1, and magnesium alloy profiles extrusion die (left and right half module 10,20 is in closure state) places on the die sinking cushion block 4 and under the suppressing action of the wedge-shaped part of die sinking drift 3 left and right half module 10,20 opened.
Extrude die-cushion 7 and be the cover tubular, extrude on the platform 5 that die-cushion 7 places forcing press 1, right half module 20 places to be extruded on the die-cushion 7 and under the suppressing action of extruding drift 6 the residual magnesium alloy 30 of right half module tap hole is extruded downwards, drops in the tube chamber of extruding die-cushion 7.
The method for cleaning of magnesium alloy profiles extrusion die provided by the invention is as follows:
As shown in Figure 3,
(1) die sinking cushion block 4 is placed on the platform 5 of forcing press 1, the magnesium alloy profiles extrusion die is placed die sinking cushion block 4;
(2) die sinking drift 3 is installed on the slide block 2 of forcing press 1, the wedge-shaped part of die sinking drift 3 lower ends is aimed at the interface place of the left and right half module 10,20 of magnesium alloy profiles extrusion die;
(3) the slide block 2 drive die sinking drifts 3 of forcing press are moved down, open the left and right half module 10,20 of magnesium alloy profiles extrusion die;
As shown in Figure 4,
(4) remove die sinking cushion block 4,, extrude die-cushion 7 and be the cover tubular, the right half module 20 that fills up residual magnesium alloy 30 in the tap hole is placed extrude on the die-cushion 7 extruding on the platform 5 that die-cushion 7 places forcing press 1;
(5) install on the slide block 2 of forcing press and extrude drift 6, the profile of extruding the lower end of drift 6 and the tap hole 50 on the right half module 20 is suitable;
(6) slide block 2 of forcing press is driven extrude drift 6 and move down, magnesium alloy 30 residual in the tap hole with right half module 20 is extruded, and drops in the tube chamber of extruding die-cushion 7.
Method with the cleaning extrusion die that has magnesium alloy profiles now is compared, and method provided by the invention has following advantage:
(1) saved the energy that one section aluminium bar and the alkali that consumes when boiling mould and heating buck consume.
When (2) having prevented to eject magnesium alloy, remain in aluminium in the mould, simplified the troublesome operation of cleaning mould the pollution of mould with aluminium bar.
(3) magnesium alloy that clears can remelting, utilization again.
(4) technology is simple, by original use aluminium bar eject magnesium alloy, again cook off by buck remove residual aluminium, last die sinking cleaning becomes directly die sinking of machinery, extrudes residual magnesium alloy, reduce production costs.
(5) this method does not re-use buck and boils, and can not endanger the healthy of workman, does not pollute the environment.
The present invention is not limited to above-mentioned preferred forms, and anyone should learn the structural change of making under enlightenment of the present invention, and every have identical or close technical scheme with the present invention, all falls within protection scope of the present invention.

Claims (4)

1. the cleaning plant of magnesium alloy profiles extrusion die, described magnesium alloy profiles extrusion die is formed by left half module and right half module assembly, and described right half module is provided with tap hole, it is characterized in that, and described cleaning plant comprises:
Forcing press;
Extrude drift, its upper end is provided with and is used for and the fixing interface of the slide block of described forcing press, and the shape of the tap hole on lower end and the described right half module is suitable;
Extrude die-cushion, be the cover tubular, described extruding on the platform that die-cushion places described forcing press, described right half module place described extrude on the die-cushion and under the described suppressing action of extruding drift, the residual magnesium alloy of described right half module tap hole extruded drop in the described tube chamber of extruding die-cushion.
2. the cleaning plant of magnesium alloy profiles extrusion die as claimed in claim 1, it is characterized in that also comprising die sinking drift and die sinking cushion block, the upper end of described die sinking drift is equipped with and is used for and the fixing interface of the slide block of described forcing press, the lower end is provided with and the wedge-shaped part that is used to open described left half module and right half module, the upper surface of described die sinking cushion block is provided with and the suitable arc groove of the outer circumference surface of described magnesium alloy profiles extrusion die, described die sinking cushion block places on the platform of described forcing press, and described magnesium alloy profiles extrusion die places on the described die sinking cushion block and open a described left side under the suppressing action of the wedge-shaped part of described die sinking drift, right half module.
3. the method for cleaning of magnesium alloy profiles extrusion die is characterized in that may further comprise the steps:
A10, will process magnesium alloy profiles the magnesium alloy profiles extrusion die left and right half module separately;
A20, on the platform of forcing press, put the right half module pad of cover tubular, the right half module that fills up magnesium alloy in the tap hole placed extrude on the die-cushion, tap hole be positioned at described extrude die-cushion directly over;
A30, install on the slide block of forcing press and extrude drift, the profile of extruding the lower end of drift and the tap hole on the right half module is suitable;
A40, the slide block of forcing press is driven extrude drift and move down, magnesium alloy residual in the tap hole with right half module is extruded, and drops in the described tube chamber of extruding die-cushion.
4. the method for cleaning of magnesium alloy profiles extrusion die as claimed in claim 3 is characterized in that, steps A 10 may further comprise the steps:
A101, on the platform of forcing press, place the die sinking cushion block, the magnesium alloy profiles extrusion die is placed the die sinking cushion block;
A102, the die sinking drift is installed on the slide block of forcing press, the wedge-shaped part of die sinking drift lower end is aimed at the interface place of the left and right half module of magnesium alloy profiles extrusion die;
A103, make the slide block of forcing press drive the die sinking drift to move down, open the left and right half module of magnesium alloy profiles extrusion die.
CN2011100728867A 2011-03-25 2011-03-25 Magnesium alloy profile extrusion die cleaning device and method Pending CN102198456A (en)