CN101564930A - Bailer liquid - Google Patents

Bailer liquid Download PDF

Info

Publication number
CN101564930A
CN101564930A CNA2009101077230A CN200910107723A CN101564930A CN 101564930 A CN101564930 A CN 101564930A CN A2009101077230 A CNA2009101077230 A CN A2009101077230A CN 200910107723 A CN200910107723 A CN 200910107723A CN 101564930 A CN101564930 A CN 101564930A
Authority
CN
China
Prior art keywords
paper
jin
bailer liquid
water
bailer
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
CNA2009101077230A
Other languages
Chinese (zh)
Other versions
CN101564930B (en
Inventor
陈琳
李建兵
李昌盛
郭迎兵
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Shenzhen Hua Xin Colour-Printing & Platemaking Co Ltd
Original Assignee
Shenzhen Hua Xin Colour-Printing & Platemaking Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Shenzhen Hua Xin Colour-Printing & Platemaking Co Ltd filed Critical Shenzhen Hua Xin Colour-Printing & Platemaking Co Ltd
Priority to CN2009101077230A priority Critical patent/CN101564930B/en
Publication of CN101564930A publication Critical patent/CN101564930A/en
Application granted granted Critical
Publication of CN101564930B publication Critical patent/CN101564930B/en
Expired - Fee Related legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

The invention is suitable for the field of printing technique, and provides bailer liquid containing water 70-80 parts, isopropanol 20-30 parts and fountain solution 0.5-2 parts by mass of bailer liquid. Compared with the completed product 'soybean' printing ink, the bailer liquid provided by the invention is produced by a simple and convenient method which reduces cost and improves efficiency, at the same time the bailer liquid can quickly dry the printing ink, prevent stain, smear and set-off in the printing process of metal paper, iridescent paper, butter paper, munken paper, writing paper or the like.

Description

A kind of Bailer liquid
Technical field
The invention belongs to printing technology, relate in particular to a kind of Bailer liquid.
Background technology
Offset printing is to print according to oil, the not miscible basic principle of water.Printing figure message part oleophylic is scolded water, the hydrophilic China ink of refusing of blank parts.In the offset printing process, space of a whole page moisture is crossed conference and is caused the printing site to send out sky, roller stripping, and color is unglazed, and level is fuzzy, texture is poor, the trace rate of drying waits slowly.Space of a whole page moisture is too small, phenomenons such as the site is unintelligible, scumming, dirty version can occur.Therefore, in offset printing process, it is very crucial how using Bailer liquid.At present, the Bailer liquid proportioning of using in the typography is: the water of 81~90 mass parts, the fountain solution of the isopropyl alcohol of 8~12 mass parts and 3~5 mass parts.The water of 86 mass parts commonly used in the practice, the fountain solution preparation Bailer liquid of the isopropyl alcohol of 10 mass parts and 4 mass parts, still, this Bailer liquid is oversize to drying times such as metal foiled paper, iridescent paper, tracing paper, the willing paper of illiteracy, writing papers, and rub easily and spend, bedraggle, loss is big especially.Though existing a kind of finished product " soybean " printing ink can head it off, this printing ink is relatively more expensive, and each production need to change printing ink, has wasted the time of a lot of carwash, and cost height, efficient are low.
Summary of the invention
The purpose of the embodiment of the invention is to provide a kind of Bailer liquid, be intended to solve existing Bailer liquid to metal foiled paper, iridescent paper, tracing paper, illiteracy agree paper, writing paper etc. should the brush process in, the ink setting time is oversize, and rub easily the flower, bedraggle the problem that loss is big.
The embodiment of the invention is achieved in that
A kind of Bailer liquid in mass parts, contains 0.5~2 part of 70~80 parts in water, 20~30 parts of isopropyl alcohols and fountain solution.
Compared with prior art, technique scheme adopts the water of 70~80 mass parts, the isopropyl alcohol of 20~30 mass parts and the fountain solution preparation Bailer liquid of 0.5~2 mass parts, metal foiled paper, iridescent paper, tracing paper, illiteracy are being agree in the printing process of paper, writing paper etc., with respect to using finished product " soybean " printing ink, method is easy, has reduced cost, has improved efficient, printing ink is done soon, have can prevent sticking flower, spend the end, the advantage of set-off.
The specific embodiment
In order to make purpose of the present invention, technical scheme and advantage clearer,, the present invention is further elaborated below in conjunction with embodiment.Should be appreciated that specific embodiment described herein only in order to explanation the present invention, and be not used in qualification the present invention.
It is compared with prior art a kind of that the embodiment of the invention provides, metal foiled paper, iridescent paper, tracing paper, illiteracy are being agree in the printing process of paper, writing paper etc., and cost is low, the efficient height, printing ink is done soon, have can prevent sticking flower, spend the end, the Bailer liquid of advantage such as set-off.
Particularly, the Bailer liquid that the embodiment of the invention provides in mass parts, contains 0.5~2 part of 70~80 parts in water, 20~30 parts of isopropyl alcohols and fountain solution.Wherein, water can be pure water, running water, well water or river, and fountain solution is this area fountain solution commonly used, and generally speaking, the fountain solution of buying on the market all can.The mass parts of preferred water is 72~77, the mass parts of isopropyl alcohol be 20~30 and the fountain solution quality part be 1~1.5.More preferably, the mass ratio of the quality of the quality of water, isopropyl alcohol and fountain solution is 75: 24: 1.The Bailer liquid that uses the embodiment of the invention to provide, metal foiled paper, iridescent paper, tracing paper drying time is 1 day; Cover agreeing paper, book paper, tracing paper drying time is 3.5-8 hour.
Comparative Examples 1
In to the printing process of metal foiled paper, iridescent paper, tracing paper, use the Bailer liquid of following proportioning to pour the printing machine water tank into:
86 jin of pure water
10 jin of isopropyl alcohols
4 jin of fountain solutions
In water tank, test, the isopropyl alcohol test concentrations be 9% (water tank working environment difference, pour into Bailer liquid concentration behind the water tank compare can change before pouring into), electrical conductivity is 900us, pH value is 4.8.
Effect: 10 days drying times of metal foiled paper, iridescent paper drying time is 8 days, and be 5 days the drying time of tracing paper, and all rubs and phenomenon such as spend, bedraggle to take place.
Comparative Examples 2
In to the printing process that covers willing paper, book paper, use the Bailer liquid of following proportioning to pour the printing machine water tank into:
86 jin in running water
10 jin of isopropyl alcohols
4 jin of fountain solutions
Test in water tank, testing conductivity is 900us, and pH value is 4.8, and isopropyl alcohol concentration is 9%.
Effect: cover to agree 2 days drying times of paper, book paper drying time is 3 days, and all rubs and the phenomenon generation such as spend, bedraggle.
Embodiment 1
In to the printing process of metal foiled paper, iridescent paper, tracing paper, use the Bailer liquid of following proportioning to pour the printing machine water tank into:
75 jin of pure water
24 jin of isopropyl alcohols
1 jin of fountain solution
Test in water tank, testing conductivity is 480us, and pH value is 7.5, isopropyl alcohol concentration 19%.
Effect: 18 hours drying times of metal foiled paper, iridescent paper drying time is 12 hours, and be 8 hours the drying time of tracing paper, does not have to rub and the phenomenon generation such as spend, bedraggle.
Embodiment 2
In to the printing process that covers willing paper, book paper, use the Bailer liquid of following proportioning to pour the printing machine water tank into:
75 jin of pure water
24 jin of isopropyl alcohols
1 jin of fountain solution
Test in water tank, testing conductivity is 480us, and pH value is 7.4, and isopropyl alcohol concentration is 19%.
Effect: cover to agree 4 hours drying times of paper, book paper drying time is 4 hours, does not all have to rub and the phenomenon generation such as spends, bedraggle.
Embodiment 3
In to the printing process of metal foiled paper, iridescent paper, tracing paper, use the Bailer liquid of following proportioning to pour the printing machine water tank into:
77 jin in running water
21 jin of isopropyl alcohols
2 jin of fountain solutions
Test in water tank, testing conductivity is 500us, and pH value is 7.3, isopropyl alcohol concentration 17%.
Effect: 19 hours drying times of metal foiled paper, iridescent paper drying time is 13 hours, and be 9 hours the drying time of tracing paper, does not have to rub and the phenomenon generation such as spend, bedraggle.
Embodiment 4
In to the printing process that covers willing paper, book paper, use the Bailer liquid of following proportioning to pour the printing machine water tank into:
77 jin in running water
21 jin of isopropyl alcohols
2 jin of fountain solutions
Test in water tank, testing conductivity is 500us, and pH value is 7.3, isopropyl alcohol concentration 17%.
Effect: cover to agree 5 hours drying times of paper, book paper drying time is 6 hours, does not have to rub and the phenomenon generation such as spend, bedraggle.
Embodiment 5
In to the printing process of metal foiled paper, iridescent paper, tracing paper, use the Bailer liquid of following proportioning to pour the printing machine water tank into:
76.5 jin in running water
23 jin of isopropyl alcohols
0.5 jin of fountain solution
Test in water tank, testing conductivity is 490us, and pH value is 7.5, isopropyl alcohol concentration 18%.
Effect: 17 hours drying times of metal foiled paper, iridescent paper drying time is 11 hours, and be 10 hours the drying time of tracing paper, does not have to rub and the phenomenon generation such as spend, bedraggle.
Embodiment 6
In to the printing process that covers willing paper, book paper, use the Bailer liquid of following proportioning to pour the printing machine water tank into:
76.5 jin in running water
23 jin of isopropyl alcohols
0.5 jin of fountain solution
Test in water tank, testing conductivity is 490us, and pH value is 7.5, isopropyl alcohol concentration 18%.
Effect: cover to agree 3.5 hours drying times of paper, book paper drying time is 5 hours, does not have to rub and the phenomenon generation such as spend, bedraggle.
Embodiment 7
In to the printing process of metal foiled paper, iridescent paper, tracing paper, use the Bailer liquid of following proportioning to pour the printing machine water tank into:
80 jin in running water
20 jin of isopropyl alcohols
0.5 jin of fountain solution
Test in water tank, testing conductivity is 450us, and pH value is 7.2, isopropyl alcohol concentration 16%.
Effect: 17 hours drying times of metal foiled paper, iridescent paper drying time is 15 hours, and be 12 hours the drying time of tracing paper, does not have to rub and the phenomenon generation such as spend, bedraggle.
Embodiment 8
In to the printing process that covers willing paper, book paper, use the Bailer liquid of following proportioning to pour the printing machine water tank into:
80 jin in running water
20 jin of isopropyl alcohols
0.5 jin of fountain solution
Test in water tank, testing conductivity is 400us, and pH value is 7.0, isopropyl alcohol concentration 16%.
Effect: cover to agree 3.5 hours drying times of paper, book paper drying time is 4.5 hours, does not have to rub and the phenomenon generation such as spend, bedraggle.
Embodiment 9
In to the printing process of metal foiled paper, iridescent paper, tracing paper, use the Bailer liquid of following proportioning to pour the printing machine water tank into:
72 jin in running water
30 jin of isopropyl alcohols
1 jin of fountain solution
Test in water tank, testing conductivity is 520us, and pH value is 6.8, isopropyl alcohol concentration 22%.
Effect: 17 hours drying times of metal foiled paper, iridescent paper drying time is 15 hours, and be 12 hours the drying time of tracing paper, does not have to rub and the phenomenon generation such as spend, bedraggle.
Embodiment 10
In to the printing process that covers willing paper, book paper, use the Bailer liquid of following proportioning to pour the printing machine water tank into:
72 jin in running water
30 jin of isopropyl alcohols
1 jin of fountain solution
Test in water tank, testing conductivity is 520us, and pH value is 6.8, isopropyl alcohol concentration 22%.
Effect: cover to agree 3.5 hours drying times of paper, book paper drying time is 4.5 hours, does not have to rub and the phenomenon generation such as spend, bedraggle.
Embodiment 11
In to the printing process of metal foiled paper, iridescent paper, tracing paper, use the Bailer liquid of following proportioning to pour the printing machine water tank into:
72 jin in running water
30 jin of isopropyl alcohols
1.5 jin of fountain solutions
Test in water tank, testing conductivity is 510us, and pH value is 6.5, isopropyl alcohol concentration 21%.
Effect: 17 hours drying times of metal foiled paper, iridescent paper drying time is 15 hours, and be 12 hours the drying time of tracing paper, does not have to rub and the phenomenon generation such as spend, bedraggle.
Embodiment 12
In to the printing process that covers willing paper, book paper, use the Bailer liquid of following proportioning to pour the printing machine water tank into:
72 jin in running water
30 jin of isopropyl alcohols
1.5 jin of fountain solutions
Test in water tank, testing conductivity is 510us, and pH value is 6.5, isopropyl alcohol concentration 21%.
Effect: cover to agree 3.5 hours drying times of paper, book paper drying time is 4.5 hours, does not have to rub and the phenomenon generation such as spend, bedraggle.
Adopt river, well water according to the preparation of the ratio in the various embodiments described above Bailer liquid, the basic no change of test effect.
The above only is preferred embodiment of the present invention, not in order to restriction the present invention, all any modifications of being done within the spirit and principles in the present invention, is equal to and replaces and improvement etc., all should be included within protection scope of the present invention.

Claims (5)

1, a kind of Bailer liquid in mass parts, contains 0.5~2 part of 70~80 parts in water, 20~30 parts of isopropyl alcohols and fountain solution.
2, Bailer liquid as claimed in claim 1, wherein, electrical conductivity is 300-520us, pH value is 5~8.
3, Bailer liquid as claimed in claim 1, wherein, the mass parts of water is 72~77, the mass parts of isopropyl alcohol be 20~30 and the fountain solution quality part be 1~1.5.
4, Bailer liquid as claimed in claim 2, wherein, the mass ratio of the quality of water, the quality of isopropyl alcohol and fountain solution is 75: 24: 1.
5, as each described Bailer liquid of claim 1~4, wherein, water is pure water, running water, well water or river.
CN2009101077230A 2009-05-26 2009-05-26 Bailer liquid Expired - Fee Related CN101564930B (en)