CN100389924C - 一种p91钢焊接方法 - Google Patents

一种p91钢焊接方法 Download PDF

Info

Publication number
CN100389924C
CN100389924C CNB200510012560XA CN200510012560A CN100389924C CN 100389924 C CN100389924 C CN 100389924C CN B200510012560X A CNB200510012560X A CN B200510012560XA CN 200510012560 A CN200510012560 A CN 200510012560A CN 100389924 C CN100389924 C CN 100389924C
Authority
CN
China
Prior art keywords
welding
steel
layer
heating
temperature
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Expired - Fee Related
Application number
CNB200510012560XA
Other languages
English (en)
Other versions
CN1721118A (zh
Inventor
王宝才
王志伟
王迎军
焦荣格
孙芳
何生贵
刘石群
扬全义
王全印
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
WELDING TRAINING CENTER SHIJIAZHUANG ELECTRIC POWER INDUSTRY SCHOOL
Original Assignee
WELDING TRAINING CENTER SHIJIAZHUANG ELECTRIC POWER INDUSTRY SCHOOL
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by WELDING TRAINING CENTER SHIJIAZHUANG ELECTRIC POWER INDUSTRY SCHOOL filed Critical WELDING TRAINING CENTER SHIJIAZHUANG ELECTRIC POWER INDUSTRY SCHOOL
Priority to CNB200510012560XA priority Critical patent/CN100389924C/zh
Publication of CN1721118A publication Critical patent/CN1721118A/zh
Application granted granted Critical
Publication of CN100389924C publication Critical patent/CN100389924C/zh
Expired - Fee Related legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

本发明提供一种P91钢焊接方法,基本步骤包括预热,打底焊接,填充焊接,保温热处理,其特征在于:采用TGS-9Cbφ2.4焊丝打底,C9MVφ2.5,C9MVφ3.2焊条填充焊接,填充焊接的参数选择为:焊接电流75-140A,每层焊接时间6-21分钟,焊接预热温度150℃,焊接层间温度200-300℃。本发明的技术进步效果表现在:利用加大焊接电流,提高焊接速度来降低线能量的工艺方法,改变了行业上普遍采用小电流了降低线能量的做法,提高焊接速度近一倍;改变层道布置,减少同层焊道,降低焊层厚度,不但便于操作,还克服了因焊道多造成的焊道厚度加大而形成的死角,有效防止焊接缺陷的产生,利用层间回火效应,改善焊缝金属组织和性能;达到焊接操作标准化,焊接过程程序化,技术工人便于培训和管理。

Description

一种P91钢焊接方法
技术领域
本发明涉及到一种P91钢焊接工艺方法,属于特种钢管焊接技术领域。
背景技术
P91钢是一种新型的高合金耐热钢材,以其高温持久强度和抗蠕变断裂性能优异被广泛采用,与T22钢相比在相同温度、压力的条件下,管子壁厚减薄50%,减少了结构重量;与奥氏体钢相比,膨胀系数小,并改善了热传导性,价格也相对便宜;不论从使用性能,还是经济性,都表现出了它的优越性,作为高温过热器联箱、主蒸汽管道等高温高压管道的首选及替代钢种。P91钢焊接难度比较大,主要表现在容易出现焊缝背面氧化,焊接接头脆化冷裂纹,冲击韧性低等问题,主要原因是在施焊过程中,焊接线能量较大,层间温度高,从而造成层间组织过热,产生魏氏组织,粗大晶粒和网状晶界,这些组织均容易产生裂源,形成裂纹并扩展,导致焊缝的冲击韧性下降。为了减小线能量,现有技术通常的做法是小电流,慢速施焊,生产效率低,对焊工要求技术水平高,P91钢管的焊接周期大约24-30小时。因此,选择P91钢的焊接参数,制定适用于生产现场的焊接工艺条件,具有重要的现实意义和经济价值。
发明内容
本发明的目的在于提供一种标准化的P91钢焊接方法,利用工艺参数的合理选择降低线能量,防止焊接缺陷的产生和提高焊接速度。
本发明的技术方案是这样实现的:这种P91钢焊接方法,基本步骤包括预热,打底焊接,填充焊接,保温热处理,其特征在于:采用TGS-9Cbφ2.4焊丝打底,C9MVφ2.5,C9MVφ3.2焊条填充焊接,填充焊接的参数选择为:焊接电流75-140A,每层焊接时间6-21分钟,焊接预热温度150℃,焊接层间温度200-300℃。
所述的P91钢焊接方法所述的焊接参数的选择是:根据填充层逐渐加厚选择从75-140A依次递增焊接电流,每层填充焊接时间6-11分钟,第15层后焊接电流降至120A,填充焊接时间11-21分钟。
所述的P91钢焊接方法的焊接参数的选择是:填充焊接时间是10小时,降温到100-150℃保持2小时。
所述的P91钢焊接方法的焊接过程中需要升温的速度≤150℃/h。
所述的P91钢焊接方法的保温热处理方法是:
A、焊后热处理的升、降温速度≤150℃/h;
B、加热温度为760℃±5℃,保温时间为4小时;
C、降温至200℃时,冷却至室温。
D、加热带宽度300mm,保温宽度≥800mm,钢管内壁加热范围两端用保温毛毡封堵,防止空气对流。
所述的P91钢焊接方法,其特征在于焊接坡口为U形。
本发明的技术进步效果表现在:1利用加大焊接电流,提高焊接速度来降低线能量的工艺方法,改变了普遍采用小电流降低线能量的做法,提高焊接速度近一倍;2、改变层道布置,减少同层焊道,降低焊层厚度,不但便于操作,还克服了因焊道多造成的焊道厚度加大而形成的死角,有效防止焊接缺陷的产生,利用层间回火效应,改善焊缝金属组织和性能;4、达到焊接操作标准化,焊接过程程序化,技术工人便于培训和管理。
经济效益分析:1、焊接速度提高了近一倍,对于火力发电厂而言,效益可观。2、从回火温度和恒温时间提高1/3,既保证了焊接接头的性能指标,又节约了时间、同样增加焊接劳动生产率。
附图说明
图1为焊接坡口的形状及尺寸示意图
图2为焊层、焊道示意图
图3为预热、打底、填充焊接和热处理过程规范曲线图
具体实施方式
下面结合P91(SA335-P91)钢管具体焊接实例和附图,详细说明本发明的一种实施方式:
本发明的T91钢焊接操作方法如下:
1、机具与焊接材料
①焊接设备应选用特性良好的逆变式焊机;
②焊丝:TGS-9Cbφ2.4,焊条:C9MVφ2.5,C9MVφ3.2
2、坡口制备
①坡口形状及尺寸(mm)见图1;
②坡口制备时以机械方式加工;
③坡口及内外壁两侧20mm范围内锈、油、垢等污物清理干净,露出金属光泽。
3、焊接方法
①试件焊接为水平位置固定,由两个焊工对称施焊,以保持受热均衡;
②打底:采用手工钨极氩弧焊TGS-9Cbφ2.4焊丝打底;
③填充采用手工焊条C9MVφ2.5,C9MVφ3.2电弧焊填充、盖面的组合焊接;
④预热,焊前采取预热措施,减小温度梯度,防止冷裂纹的发生;打底焊时,预热温控制在150℃,打底焊完成后,填充焊接预热温度控制在250-300℃进行填充。
⑤填充焊接:焊接过程参数见表1,施焊层道见图2
表1
Figure C20051001256000061
4、焊后热处理
焊接完成后,试件缓冷降温至100~150℃,保温1-2小时,待马氏体转变完成后,进行焊后热处理。为适应现场需要,采用柔性陶瓷电阻远红外加热带,微电脑自动控温仪按设定程序控温,自动记录。升、降温速度控制在150℃/h;温度升至760℃±5℃,恒温4小时;加热带宽度300mm,保温宽度800mm以上,管内壁加热范围两端用保温毡封堵,防止空气对流,以减小内外壁温差。预热、打底、填充焊接和热处理规范曲线见图3。
5、力学性能指标见表2
Figure C20051001256000071
结论:
1、P91钢除了传统的固熔强化、沉积强化外,还通过微合金化、形变热处理及控温获得高密度位错和高度细化的晶粒,使P91钢的高温强度进一步提高,同时其韧性也获得了显著提高。由于普通焊接状态下很难实现母材的组织状态和力学性能状态,特别体现在冲击韧性值,必须依靠焊接过程适当的小线能量、薄焊层和合适的热处理工艺,来满足焊接接头的性能要求。
2、填充焊接采用小线能量、薄焊层,采取薄焊层比多焊道效果更佳:便于利用层间回火效应,便于操作控制,减少形成夹渣缺陷几率,便于提高焊接速度。
3、焊后热处理温度控制在760℃,恒温4小时(φ350×46mm)。时间短,不足以保证回火效果;时间长,牺牲钢材寿命,且性能下降。
4、本发明的P91钢焊接方法适合施工现场,解决生产需要。
上述描述仅作为本发明所述的P91钢焊接方法的一种可实施的技术方案提出,不作为对其方法本身的单一限制条件。

Claims (6)

1.一种P91钢焊接方法,基本步骤包括预热,打底焊接,填充焊接,保温热处理,其特征在于:采用TGS-9Cbφ2.4焊丝打底,C9MVφ2.5,C9MVφ3.2焊条填充焊接,填充焊接的参数选择为:焊接电流75-140A,每层焊接时间6-21分钟,焊接预热温度150℃,焊接层间温度200-300℃。
2.根据权利要求1所述的P91钢焊接方法,其特征在于所述的焊接参数的选择是:根据填充层逐渐加厚选择从75-140A依次递增焊接电流,每层填充焊接时间6-11分钟,第15层后焊接电流降至120A,填充焊接时间11-21分钟。
3.根据权利要求2所述的P91钢焊接方法,其特征在于所述的焊接参数的选择是:填充焊接时间是10小时,降温到100-150℃保持1-2小时。
4.根据权利要求3所述的P91钢焊接方法,其特征在于所述的焊接过程中需要升温的速度≤150℃/h。
5.根据权利要求3所述的P91钢焊接方法,其特征在于所述的保温热处理方法是:
A、焊后热处理的升、降温速度≤150℃/h;
B、加热温度为760℃±5℃,保温时间为4小时;
C、降温至200℃时,冷却至室温。
D、加热带宽度300mm,保温宽度≥800mm,钢管内壁加热范围两端用保温毛毡封堵,防止空气对流。
6.根据权利要求1所述的P91钢焊接方法,其特征在于焊接坡口为U形。
CNB200510012560XA 2005-06-02 2005-06-02 一种p91钢焊接方法 Expired - Fee Related CN100389924C (zh)