CA2150018C - Open cell polypropylene foam and process for making same - Google Patents

Open cell polypropylene foam and process for making same Download PDF

Info

Publication number
CA2150018C
CA2150018C CA002150018A CA2150018A CA2150018C CA 2150018 C CA2150018 C CA 2150018C CA 002150018 A CA002150018 A CA 002150018A CA 2150018 A CA2150018 A CA 2150018A CA 2150018 C CA2150018 C CA 2150018C
Authority
CA
Canada
Prior art keywords
foam
blowing agent
cell
percent
open
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Expired - Lifetime
Application number
CA002150018A
Other languages
French (fr)
Other versions
CA2150018A1 (en
Inventor
Chung P. Park
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Dow Global Technologies LLC
Original Assignee
Dow Global Technologies LLC
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Family has litigation
First worldwide family litigation filed litigation Critical https://patents.darts-ip.com/?family=22231647&utm_source=google_patent&utm_medium=platform_link&utm_campaign=public_patent_search&patent=CA2150018(C) "Global patent litigation dataset” by Darts-ip is licensed under a Creative Commons Attribution 4.0 International License.
Application filed by Dow Global Technologies LLC filed Critical Dow Global Technologies LLC
Publication of CA2150018A1 publication Critical patent/CA2150018A1/en
Application granted granted Critical
Publication of CA2150018C publication Critical patent/CA2150018C/en
Anticipated expiration legal-status Critical
Expired - Lifetime legal-status Critical Current

Abstract

Disclosed is a process for making a low density, dimensionally-stable, open-cell, extruded propylene polymer foam comprising primarily an expanded propylene polymer material wherein the foam has a blowing agent comprising greater than 85 percent by weight of one or more organic blowing agents based upon the total weight of the blowing agent. The propylene polymer material comprises more than 50 weight percent or more of propylene monomeric units based upon the total weight of the propylene polymer material. The foam has a density 96 kilograms or less per cubic meter. The foam is greater than 20 percent open cell.

Description

2~~OOIB
~~D 94/13460 PCT/US92/10934 OPEN CELL POLYPROPYLENE FOAM AND PROCESS FOR h~lAKING SAME
This invention relates to a process for making a low density, dimensionally-stable, open-cell, extruded propylene polymer foam blown with a blowing agent comprising partly or entirely of one or more organic blowing agents. The foam offers excellent cushioning properties.
Propylene polymer foams are known in the art, and are useful in many applications such as seen in U.S.
Patent No. 3,~I81,~455, 3,871,897, 3932,569, x,522,955, and X1,832,770. Such foams have been made with a wide variety of organic and inorganic blowing agents.
It would be desirable to have an open-cell, low density propylene polymer foam (96 kilograms per cubic meter or less) for use in cushioning applications.
While closed-cell polyolefin foams, most notably eth lene y polymer foams, have typically been used in such applications, it would be desirable to use an open-cell foam for environmental reasons. Open-cell foams lose blowing agent much faster than closed-cell foams. Quick ,25 release of blowing agent is important when utilizing ~I~~~1~$

volatile blowing agents, the release of which is increasingly subject to governmental regulation. Quick m release of blowing agent allows the foam manufacturer to recover all or a substantial portion of the blowing agent prior to providing the foam to the consumer.
It would be further desirable to have an open-cell, low density propylene polymer foam that is dimensionally stable. Open-cell polyolefin foams typically are more difficult to expand to low densities than corresponding closed-cell foams because they lose blowing agent more quickly. It would be desirable to have an open-cell, propylene polymer foam that affords quick release of blowing agent while achieving a high expansion.
According to the present invention, there is a low density, dimensionally-stable, open-cell, extruded propylene polymer foam comprising a propylene polymer material wherein the foam has a blowing agent comprising greater than 85 percent or more by weight of one or more organic blowing agents based upon the total weight of the blowing agent. The propylene polymer material comprises greater than 50 percent by weight propylene monomerie units based upon the weight of the propylene polymer material. The foam has a density of 96 or less kilograms per cubic meter and preferably less than 96 kilograms per cubic meter. The foam has an open cell content of more than 20 percent.
Further according to the present invention, there is a process for making a dimensionally-stable, extruded, open-cell propylene polymer foam. The process comprises the steps of (a) heating the propylene polymer .
material comprising greater than 50 weight percent c: :-. ~ ; °~ .. > ". :°: F
:. :..,:: :~ ;.:. :..3 ~,~ ;..t:: .,..,;.. ,,Y:'.~. ., :' ~s'r ; ,.
' ! ~; '.,<:: t i'~:: . .. .J.::~~ ~: ;F~t~..~. 3~: J ..>.~. . .F:....:~.
~.'~':'3,;.,. .... .,.%v3. ~.
r:; ~ tvy 3~~.','.~, ...:... '. Ff:~::p3'3:.. .~, .. .~: '. .. . ._ .1. <.:.:
'': vi ,. >
;:iC_~': f ~:~ 'r'",y : ,"!\Yy:' (1Y,,:: ',:'y '~ -: :~ ~: : f\~~k _,t,.,,. .; ,., : .~.;~:. ',.s. ~~:,.:.... .>a.~. <..J.~....<:.. ...
'~iS:'::i. ;;2',.t... .:'., ;
..i s.E ii ...... :..:.~.><,...... :.. ~'a.:~ . J .-. ... ... .. ..
~ !~ ~ '. r.: f ~ .Y , y ~ r ': )' w, :'_> r- C:'r- ,...
.. (.,,.), J . . . _. . . ~' ...,.. ,:< w .:2v.: .:.4 :~
_: :. ~.: ~ ,. .. _~. ;y~~ :~, ~ :::. ~ '::. ., ... _. ... ... p'.: .~..~. .
.~ .. .. '°~:p ~': .: __. . ;;t ~. . .. .., -r_:r '";c::.~:..~~'';.r ..(~..1.,., .?.f;~J~' ~::3:.1~ _., . .'.t::".a~w, ~:i....... .~'~ ,...... .~ .... 'p .,.:.:..3:: a~. .: : ..... ~ .:y3:::
' :) ', .'a/' G: "'. Yy'.H C'~Gai'? ;.ry;';: <..Y~;~', y~).:~. -.:) .. '.~'t: : ~~-~>,.'-.,..:.. .. ~...~.f:..:.: .c......:.).....,2 ~. .:.:.
....skc. .~~.:.;..._. <;,.. %'~~,:..: ~.'y%~ v,.......
.: .. _ _.~ _,.3 . :. w: ~ ~ ,- w ,..~i .. .:
:...:.....J.~:.,~. ".i ' _: ~~.:.'~. f.'.u ~.. _7.~ Y;.~:. .. ..... ...<<'.c<
~:. ... ':~C'~ .. j . ..: i ~.f..4...,..~...<
:~~i%i.".i:).~.t;:" '~w:':. ~.?.!~':J'f_:~J,'.~"f ::: ~'.~a f:.::~y :....
":'~".3; #::::.... ~~~i%:i~~:;, ,..;.C..,.r.,.: , . . . -,...l~,l, ~:y... ;. ;. ,..,_~.;:,~ . . :i.=~:.~.: ..
...
. . ,. .. ..: ... ,~ ."'. 1'~ y:% .. .: .. :.., .. :.v::~: :_. _. ,. .: ~~- ,~
. . .. ,>r ,. .: i f'.'' :1 ~~ .:. I 1 . ... , -..:a :-c: -r;-;.~(~.~r' ;~ ~~!-Y,",~',' :'ya.~: Y;::: :W:',~:,t::.y -i t~..~'.-.~, ._ .. . ..'. ,' .. :.) y .. . v .~. ::. ..... ... ~. ,. ~1......s., sJ ...
v.._. s.....v.~:..S.~t~:~.:~ '... .1. ,..,t,. ...'...J . ...,.,v.: ':. .~. A:' ;"' C~.~i $ ,:Y)r -: y :> ' __.t~.::.
.. . .r; ~ .. , ....... . ,Li.ki.; :~,.~~ \.. ..~.s ~~i ~~~ n' . . i . ~. . .. v .. .. ...v .. .'Cl.~. ~~ .. C..t. ~iV J :v ~.S' .,.. .. ,.. .. ,.E ..: :~,. '.: / t~.. ~. :.. . . . . wt 3, i ~i ~ ..i J Y'/
.' .~ .. ..: ..
_. ~;.r_<,. !.. - ,r :- ; : r' : Y: ; i . . '..fa'~r'. ('<:'~ ".'Y' , r'i~~~':~ .1. ;. , . ..s z:..; .... ..,......._.. ._.,..~i;'~
;>..~.~i...:~3'., .. :i:::~::..... c;
E..~ '. t.. .: ,.,..... '. <.: ~ ~ . . . . .. . :. , s J '~.: ~ t ~ .., . _., :,~ '~, C_:....: ';-1; ~: : ,~ ~ ; :; I !r .w :'?'\'~,~'.: C:.' ': ~- ~',)..
:. "~~..F~~. . . :. /~~:::'... ~'~":.:~~:.c:':.........,. ....ui~"..f;::,.
...,.:._.~-~ ...'-~E~='~3....~.. :...:......
..,_.,..~...~, .. a- f.,,-;.~!., ..,,,-'t ~,.~ .., ~:;-, :':(:, - '.'% 't ~: . t=~ : . . . r ~'. ~ i ' ! . ~" ...
~J~,~..._...t:.lL~.. :.1.~ wl;. :~.~%,. .,. "'"'~:'< ''."..,.
~~~iv_...s..i~~.'.v:....:. ., v:.,.:...... s. 3.iv.~s'C... ..G.:JSi~S~S
.......
S, #.. (.., :: >' . _...~ ...., t~ .1,.;:) .rs.;~y': ~ Y,'!;: ~' ''!;; : ~'~
C:-y~,; .., ~? :,:. f~ .f ~ Y.. y~::G>. : ' t ',.a. :~.:.:.. :.:_. v..1S.'.~ ..Jr.t...~ .~ ~-~~-~ .. " ~ ~... ~.
>(...<.'.v...,. :.CCia. _. _: $..(,!.i.'(%~: ... ~3s~....v.s.
7;~- ,..(',.., r~,.Y. r~'. i ~::'y-: ~t~: . ;c;~ iw ;-,!-;': , :ca y~
..... p. ., ....:.. ,..... _ ~ _. _:~ ~ ::..: ~:3.. .J .. .. w y~~. :,'~ ~ <._ .. t~:... :3..:_..~ ~. H ..:. X/":3,......
y.. ~.f,:f ,:: yt.w':',~ ry.r :' =;-y.,.fa : ;~r',:~t.~';;: ::) . f t~.r j l..t~::..,y'~ r:;.,_ ..r.........:...c........ .... ~:.~.:.. 5,.,...~3.:.:',~~ '~3.'::~'-'~~s.. .«i ~..........:;. ,:.f. .... ,.~...~.<.,.t:~r...~:."~ ~ i.~tvr.~ ~ . ",.,. '..
w c.;, ~"f'.:' (~;~~5 ;"('., v:'y:::~,r ':<=~'~' :) ' ~ ''> r.:-~;..... ; ;t~
;:~3.... .. .:<~..;v.~i...,.. .., .:.4. s. _ ...v ~...:...,...._:~:~' ~ ~
a~E.:.~w..'u...w . : _,.13w( . ,_".......,..~ :'3w~
7~' i=W 7, " Y ':"'f'~:' :: ry. '~,~'Y':' y,)'; '-;'f' u:: r' ~~:...~.f.... ... ......it'~CZ.i.%;. ,. .%C~.:. ....:.~_....._::v::~.::. f ,......._. ._.A....<. ci :t::_~:S.~ix-: .-"... .. ,;.<~,....:...
.. r!~ - 'Y'u:::...; f.,Y, 5 .~,;~..~y:_ r~.,.Y.,:)tar' ,( !y'(~~( y ~ :-:E).
... . . . ,, . n~' ~ ~ )_; : .,., ...!;:..
S~ly~.,~.,.,..~ $.3,i.'v": '. .. .r. .s.v.....~.:...:.. '..1.~.~
.v.~..lvv~._.,. ~. :..v:.>.n::7~.C3_~S. ~._.Cl ~.~.:.~_Es: ~~_:tm. ~~:'...v. :
....,...
L. ..
,_. Y.:..~~; <4:::c:; ..~.: =.,r. : ~.r,~ ?~ fa ~ Ca~ f~ ~-. ~..',., ..;t ~.:
, ~: ( !>.
l i.> -.sJn ~.. ........ w ..J _ ...3.:...: .. ,...,., .. "...3. . ~;:...~
..... ,.'3..x ... ...... 3.;.!..: 7 ...3. ~.-...~~;.
','_>'~':':C.; t'~.~~ C_:';,_':_>'r~' i<~. 'r,)S-':~,' :";~~
f';~,::v.7"!'..~..i5'~y.. j..~.;. ':('f:'y". , ..
.. .1:.:~...~c..~......... ~~.~, v... ,. .. .. :.. '.~3~3.CQ i f ,.. .. ,: _.
. ..-~:... .. .. ... ......:.:.t.. .s: !~ ,v s.. : ..l ,.... ~.i.~.~ 'v.:.~ ..
CJ '.
;<:....... (."_.~~~:r~lr:~ ;~,M..v>~d5~~~'~ uy '~3.~.'~:~ ;~~'t:"'~f~.
:J:~Jf.%:": ...'~3~::. .~...~I. i'l~':~ ~.3':. ~..i.~.~
~.. ~'3 F:: ". ,. ,.i'."d ,i l .'~,',: i :.: ~ <
~.'~3, ~;: ..~yw' Ty-''" ~.' r.). ",(',.': , .. .
_.: ..C .s v. ...,...s.C'. t.. ~. VJ~S.. .:.t.'...3.~..: ~:J .~ ....,_. .':rj '.~u~ ~..~.u3 ~ i'! .. -- .... :. . ..
C~ v1'.,, .,,'.Y~t . '.. J Yi:'-s .yY~;C~.. ,,%:';.. .,....11~i~
w.~.Y._.....,.t;' .,r~'~ .e.! ~;~Y:.'.: "r ..... N ~ i?~.:,y .~C:'.3v~.. ..s,.., ,~: .!.:..y .~~t::.~... v?.:~_ .:.~>,::.. ~l_ ...v~..:... , ::5...3v.. C~~..':.. ....../t~s-:..~_..i .'~Z.:_.
.,~/~:vi'$ G:: ;t.:. - r,~(: :~t!'t-Yy:". ,.Y)'i.t'~. " r~,~i. y.. .': ~y...:
~ ~t.; Y:.C:'i H:.f.:.:Y a :.~....F..,.. C....~ ...: y..,.J.'~... y .F....~.'.... ~i~.~.C~'..
.......c.EH~.......c.f.~.~r..:C''~.:'... y .~,.....rC:.'~.~:.,~....,.....s..,..
:~.:'~:~.~ :~..a-r-r.: "r: ;"',~..r~ r_: ~-y;".: yr;~>'_,'r' :~r r' ;"i.,._,-;' ~,....',. . ..'....,. . ,'...t... ~ 3~:'.NJy X3'3.... { ';. ~ .:....
....,..,..~3.c~.%. :"::fw:y ..:.3:''......:'...
:-.;~')-;.._-r,,-).. _",!'; ;C)~':? t~' ?'?t...~~: "r:'.C:x-)~ ;=%':',:.r-, :~.C:
32 ..,:.::~~ ;, ,..<< _. ~%s~.X.J~.....w,.. ,...w,; .....w::i .w..., >;::f;~~ww _....,_:Lt~:;::a. '~.':~,~
.. ~ 'k~'.Y '-~i>:: ..t'::).~'.. F<..:~? C<:',,~:.:~ ....:.,. ,...'r'' .....
vy:;:~~Y.. .a,::C~ :..:a~.< .~.'i <':~. C.%~.,-' C,:Y..' :F: Y-r-.. ~-.;.,.;,.,~, ;.': r.:';-a~ 3':t~::'.'::-"-.~ t~y ~: ;~y-. .:"y-.~:
ry-_. -;:1~1 ;:);-:Ea J ' < .. .J . . 4 ..; .. ,~....t .~ . . .. . .. ,. -. ';i s:":';:':.: :':i :
.. I'3,,~. ,.. .~ F:.~ ~. ,~ :.. .f, ;,; i"
x _. .,. .. ~. .. X
~r..",;_ ;.;'; ~;..,t ,..,.;.:: ~..; _..~_. ;~~ ' ~,_;a:'~' -a~r:wy:'~- ~
t:ay,.:
_,. ~ 3 :.'... .. , .., s. .:. _....~~ ._,... ~::::3'3.. .'.):L: f',:>.F.._.
.. ~f: :. .... .. .. ~..:. ~ ~y:'.~, ... ..
~:.~(:.7y':/' , '.Yl~'.r , ,:...f:,Y.~/..,':.t,yv~ ~ j~~;'~ ;Jr.,. ; !1" ~:s -r..,y ;a 4. j."i%
..a:.v.~l >, >s.:..s.v .3:.;v.L \ .:- J. .j S..v_ ..~::) ~ '..'l~.'4: v. ....W
r'::. ..: ~.. .':.!.::.z' ..~.~. ......:

.': 'ys ' .i .;i ... . ~ ;i ti ~~:-,-r.:,;-v; ..,~'s. .-~~,. :-;Y-yy''~,cr.~.-..i,~, Y~;~;~;~~,-,r;W' ;:~r.,.i..~._ ~,:~~ ~,,:
...: v.r~. ~.....;tyi:5..r".,~~'i ,o.!.. :,..~ ~.. ~~.~...,~.: 'r~7~;':, M. .~
.". s...~,: ~.... " . :. y/ ~..;,..".., , ........ :~,:....~. s.:.~; ,:.,"j:.i .... ,..
v:!O;'.:-'.r~~.. ':~'i~ ~:~:1~ Y 7wr;;'1'~,.Y~:~.r, tY.,~.r=.t-' '..~v?~
.:Y~~,.. . :'n,-y - S .~ .,.r., .... i,~y .:,.. i i:..7. _.. "f ....... .. ° ~ ~ .. ....._ ,:::3'.x.
C,..... ._~..C.A.......... ~.':;~<t,,~: ~.::.;..'".. .., ..
w2.I:"f:?~~.r?~.,'.. ~.'~:.4:i: '> ~ :~.,W.F ~Ji:.~-..'~i.:.~:~.i.:~.~.'v"
,.f'.:"~'L: ;~.-W :~~~ ~:t~.cx; ">ri 11~y.'_~.:.'~:.'ai:.:
.'.-,'r'N'.~~i. v~ ~.~~. iJwi~Y.:..~l~,v'.'. kiitii.i.«~ :::~' .~.r: tots, :.
~i.~ .
4- ~ ' /-1C:~'',~... ~~ . .,'7 ~7 y ,~!':::.:,.~f:y t~".,-,., ... ,.u .7..i. y.:~i,j-%. ... v"sui7'3.,.: s~.~, ~,. " ~. .. ~3 ,. '.:rz x..:.
v L~~es::: t:;.'...... .. .r. ,. .,..., .. ... ~::.. ..... ".,..:.. ,..
..._.....-.,.~:.1~:.". '.i'.:~'~.~..:~.~, i!~i.~~~~'':~.'~~,;.'~.;:.~j..\:;
5~:~,".':~..~~'~,$..C,t:Y.~r:.:...t,~;?, y .s . ., i ...iijr:.::3.,"'~ ~r,~, ~E:: ~~c?r:..~'v.~. :1C-"::r'qi%:~['~:''~.~.ctv.C.
<:.~1-'.%.~. ~_a.'. ;~.:~~L'~5 x~.iz!~Ci>..:."
~.~;,r.3. .,..,.:.~~.'.r'.. %.8.~:.C."'~c. ::'~.~...,i.,'r'w..v.'.
._.x:.i3.~Yt~'~.~'a.vC.:. .lr-'a ~~~~~';~~''.W ~1;~ rr.~.:~
'i2~~ f".C3~i _ .:.i ...
r~.~~'...::. .. f,~,.. .,,, ; _;; ~; : ,,:.~Y': ~ ' r:":~ ",. .~,.,.a.. , :--.:_a ,r.:~...:._ ..:::'~_...,f" ~" v....~,i,p-).~:" ."<'~.."'.'':i ... ~
?.i~.:,.....c.'".:.'). _. C:>-.~:' .~ ~.-...,:7 s..~ ,~.......~~ii?~ ~: <:
'~:.,.a ..
' ,..;.~~~3.~y'.d.,<-"i:3..:.;...,.'.~.i.,5~ 'iY.t'C:.T."......v"..::~'.i i.~a;;'.:c.'i'::~;~,:.'.~. , _t.i.~~.W....:.~y~ v.:J~:~:i.~ ~.i~:~':~i"~n~.:.~. i'~.''. v..:f~a~tl.~.
y'::.C?~:J tii~~'':' .. 3i.?::?
... -,,.._ _-, _.~ iv'O a .c~ ~>r:: f1~ :"~rr ~ ..Y;>.~..,; a '.. i.i : r".'. J.. J ~. ~. ~~. -' ~ i a. ~... i% ~ .i. C' .. . . ... ,r s .1 ~..,w i:
_':.'~_'.'::5.~=:~.. " ~:'?,~':j:',_v i':~~IZ~: !:<.'.~yi:.~,.i.~"t~'.;~:.'?:
~: ':i.xl.:~.?~::::.~.:.' ~~<-~~W ::~~:C~:
..

WO 94/13460 :~ ~~ '~ ~ PCT/US92/10934 and block copolymers of propylene and an olefin selected from the group consisting of ethylene, Ct~-C1p 1-olefins, and C~-C10 dienes. Propylene copolymers also include random terpolymers of propylene and 1-olefins selected from the group consisting of ethylene and C1~-C8 1-olefins. In terpolymers having both ethylene and Ct~-C8 1-olefins, the ethylene content is preferably 20 percent or less by weight. The Ct~-C1p 1-olefins include the linear and branched C1~-C10 1-olefins such as, for example, 1-butene, isobutylene, 1-pentene, 3-methyl-1-butene, 1-hexene, 3,~+-dimethyl-1-butene, 1-heptene, 3-methyl-1-hexene. Examples of Ct~-C10 dimes include 1,3-butadiene, 1,~+-pentadiene, isoprene, 1,5-hexadiene, 2,3-dimethyl-1,3-hexadiene.
Suitable non-propylenic polymers ineorporatable in the propylene polymer material include high, medium, low, and linear density polyethylenes, polybutene-1, ethylene-acrylic acid copolymer, ethylene-vinyl acetate copolymer, ethylene-propylene rubber, styrene-butadiene rubber, ethylene-ethyl aerylate copolymer, ionomer.
Also, as used herein, the propylene polymer material has a melt flow rate of between 0.05 and 50 and preferably between 0.1 and 10 according to ASTM D1238 Condition L.
The preferred propylene polymer resins for the present invention are those polypropylene resins which are branched or lightly cross-linked polymer materials.
Branching (or light cross-linking) may be obtained by those methods generally known in the art, such as chemical or irradiation branching/light cross-linking.
One such resin which is prepared as a branched/lightly cross-linked polypropylene resin prior to using the -1~-2~~oo~s ~~ 94/13460 PCT/US9Z/10934 polypropylene resin to prepare a finished polypropylene resin product and the method of preparing such a polypropylene resin 'is described in U.S. Patent No.
4,916,198. Another method to prepare branched/lightly cross-linked polypropylene resin is to introduce chemical compounds into the extruder, along with a polypropylene resin and allow the branehing/lightly cross-linking reaction to take place in the extruder.
U.S. Patent No. 4,714,716 teaches this method.
Suitable branching/crosslinking agents for use in extrusion reactions have been found to include azido and vinyl functional silanes, organic peroxides and multifunctional vinyl monomers.
The blowin a ent will com rise g g p greater than 85 percent by weight and more preferably greater than 90 percent by weight, and most preferably entirely one or more volatile organic agents based upon the total weight of the blowing agent. Organic blowing agents include aliphatic hydrocarbons having 1-9 carbon atoms, halogenated aliphatic hydrocarbons, having 1-4 carbon atoms, and aliphatic aleohols having 1-3 carbon atoms.
Aliphatic hydrocarbons include methane, ethane, propane, n-butane, isobutane, n-pentane, isopentane, neopentane.
Among halogenated hydrocarbons, fluorinated hydrocarbons are preferred. Examples of fluorinated hydrocarbon include methyl fluoride, perfluoromethane, ethyl fluoride, 1,1-difluoroethane (HFC-152~a), 1,1,1-trifluoroethane (HFC-143a), 1,1,1,2-tetrafluoro-ethane (HFC-134a), pentafluoroethane, perfluoroethane, 2,2-difluoropropane, 1,1,1-trifluoropropane, perfluoropropane, perfluorobutane, perfluorocyclobutane.
Partially halogenated chlorocarbons and chlorofluorocarbons for use in this invention include WO 94/13460 ~ ~ ~ ~ ~ ~ ~ PCT/US92/10934 methyl chloride, methylene chloride, ethyl chloride, 1,1,1-trichloroethane, 1,1-dichloro-1-fluoroethane (HCFC-141b), 1-chloro-1,1-difluoroethane (HCFC-1~42b), 1,1-dichloro-2,2,2-trifluoroethane (HCFC-123) and 1-ehloro-1,2,2,2-tetrafluoroethane (HCFC-124). Fully halogenated chlorofluorocarbons include trichloromonofluoromethane (CFC-11), dichlorodifluoromethane (CFC-12), trichlorotrifluoroethane (CFC-113), dichlorotetrafluoroethane (CFC-114), chloroheptafluoropropane, and dichlorohexafluoropropane.
Fully halogenated ehlorofluorocarbons are not preferred due to their ozone depletion potential. Aliphatic aleohols include methanol, ethanol, n-propanol, and isopropanol. A most preferred organic blowing agent is a mixture of HCFC-1~42b and ethyl chloride.
The blowing agent may comprise in minor proportion (that is less than 15 weight percent) one or more inorganic blowing agents or chemical blowing agents. Suitable inorganic blowing agents useful in making the foams of the present invention include carbon dioxide, nitrogen, argon, water air, nitrogen, and helium. Chemical blowing agents include azodiearbonamide, azodiisobutyro-nitrile, benzenesulfonhydrazide, ~4,~+-oxybenzene sulfonyl-semicarbazide, p-toluene sulfonyl semi-carbazide, barium azodicarboxylate, N,N'-dimethyl-N,N'-dinitrosoterephthalamide, and trihydrazino triazine.
The amount of blowing agent incorporated into the polymer melt to make a foam-forming polymer gel is preferably from 0.05 to 0.5, and most preferably from 0.08 to 0.X10 gram moles per hundred grams of polymer.

215po~~
~'O 94/13460 PCT/US92/10934 The present foam is greater than 20 percent open cell and preferably from 30 to 70 percent open cell according to ASTM D2856-A. The open cell foams provide a high degree of resiliency normally seen only in closed cell foams.
The present foam has the density of 96 or less kilograms per cubic meter and most preferably less than X48 kilograms per cubic meter. The foam has an average cell size of 3 millimeters or less and preferably 2 millimeters or less according to ASTM D3576.
The present foam may be made in any cross-sectional size or configuration such as foam sheet or plank, but are particularly useful in making plank foam having a major dimension in cross-section of 5 centimeters or more or a cross-sectional area of 10 square centimeters or more.
The present foam is preferably substantially non-erosslinked. The term non-crosslinked is inclusive however, of the slight degree of erosslinking which may occur naturally without the use of erosslinking agents.
The present foam has the average cell wall thickness of less than 35, preferably less than 25, and most preferably less than 15 micrometers according to the formula below. It is believed that blowing agents diffuse out more rapidly from thinner cell walls than thicker ones providing more effective quenching and timely stiffening of the cell walls. As a result, the bubbles become more effectively stabilized. In addition, the thin cell walls provide greater resiliency to the cellular material. The thickness of the cell wall may be calculated approximately from the foam ~~5a~1.8 .:

density and cell size by the use of the following equation (1):
t = 0 . X16 D /B ( 1 ) where t is the thickness of cell walls in micrometers (g) and; D is cell size in ~ and B, the expansion ratio of the cellular body. Since the expansion ratio, B, can be equated the ratio of polymer density (pp) to foam density (pf), the thickness of the cell wall may be represented by equation (2):
t = (0.~+6/pp)p~ (2) For example, for a polypropylene resin having 900 kg/m3 density to have cell wall thickness less than or equal to 35 micrometers:
pfD ~ X1.28 pcf~mm (68.5 kg/m3~mm) (3) preferably, less than or equal to 25 micrometers pfD ~ 3. 06 pcf~mm 048 . 9 kg/m3~mm) ( ~ ) most preferably, less than or equal to 15 micrometers pfD ~ 1.83 pef~mm (29.4 kg/m3~mm) (5) It was found that a resin having a relatively high melt elasticity is more readily expanded to a good quality foam having a high level of open cells and meeting the foamability criterion as represented by equations (3) through (5). The elasticity of a polymer melt relative to its viscosity may be represented by tan s, which is the ratio of the loss modulus to the storage modulus. Since it is desirable to have a resin with relatively greater melt elasticity than viscosity, a polypropylene resin having a relatively small~tan s is preferred. Tan S is determined with a mechanical _g_ ~I~~~18 ~O 94/13460 PCTIUS92110934 spectrometer, such as model RDS-800, available from Rheometrics, Inc. in Piscataway, New Jersey, USA. Tan value is determined at 190°C and one radian per second oscillating frequency with a specimen of 2.5 mm thickness and 25 mm diameter. Additional details regarding determination of tan s are seen at U.S. Serial No. 07/716,034 filed June 17, .1991.
The present propylene polymer foam is generally prepared by heating a propylene polymer material to form a lasticized or melt P polymer material, incorporating therein a blowing agent to form a foamable gel, and extruding the gel through a die to form the foam product. The blowing agent may be incorporated or mixed into the plastic melt by any means known in the art such as with an extruder, mixer, blender, or the like. Prior to mixing with the blowing agent, the plastic material is heated to a temperature at or above the glass transition temperature or the melting point of the plastic material. The blowing agent is mixed with the plastic melt at an elevated pressure sufficient to prevent substantial expansion of the melt and to generally disperse the blowing agent homogeneously within the melt. Optionally, a nucleating agent is blended in the polymer melt. The feeding rate of blowing agent and nucleator are adjusted to achieve a relatively low density foam and small cell size, which results in a foam having thin cell walls. After incorporation of the blowing agent, the foamable gel is typically cooled to a lower temperature to optimize physical characteristics, including the open cell structure, of the foam product. The gel is then extruded through a die of desired shape to a zone of lower or reduced pressure to form the foam product. The _g_ WO 94/13460 ~ 1 ~ o ~ ~ $ PCT/US92110934 zone of lower pressure is at a pressure lower than that in which the foamable gel is maintained prior to extrusion through the die. The lower pressure may be superatmospheric or subatmospheric (vacuum), but is preferably at an atmospheric level.
It is also possible to add various additives such as inorganic fillers, pigments, antioxidants, acid scavengers, ultraviolet absorbers, flame retardants, processing aids, extrusion aids.
Preferred nucleating agents include inorganic substances such as calcium carbonate, talc, clay, titanium oxide, silica, barium sulfate, diatomaceous earth, mixtures of citric acid and sodium bicarbonate.
The amount of nucleating agent employed may range from 0.01 to 5 parts by weight per hundred parts by weight of a polymer resin. The preferred range is from 0.1 to 3 parts by weight.
Other suitable processes for making the present foam are a coalesced strand foam process as described in U.S. Patent No. 4,821,720 and an accumulating extrusion process described in U.S. Patent No. X1,323,528.
U.S. Patent No. 4,82+,720 describes a method for making a closed cell foam structure comprising a plurality of coalesced extruded strands or profiles by extrusion foaming of a molten thermoplastic composition utilizing a die containing a multiplicity of orifices.
The orifices are so arranged such that the contact between adjacent streams of the molten extrudate occurs during the foaming process and the contacting surfaces adhere to one another with sufficient adhesion to result in a unitary structure. The individual strands of ~~O 94/13460 PCT/US92/10934 coalesced polyolefin foam should remain adhered into a unitary structure to prevent strand delamination under stresses encountered in preparing, shaping, and using the foam.
In U.S. Patent No. X1,323,528, low density, elongated cellular bodies having large lateral cross-sectional areas are prepared by: 1) forming, under pressure, a mixture of a thermoplastic polymer and a blowing agent, with the mixture having a temperature at which the viscosity of the mixture is sufficient to retain the blowing agent when the mixture is allowed to expand; 2) extruding the mixture into a holding zone maintained at a temperature and pressure which does not allow the mixture to foam, the holding zone having an outlet die defining an orifice opening into a zone of lower pressure at which the mixture foams, and an openable gate closing the die orifice; 3) periodically opening the gate; ~4) substantially concurrently applying mechanical pressure by a movable ram on the mixture to eject the mixture from the holding zone through the die orifice into the zone of lower pressure, at a rate greater than that at which substantial foaming in the die orifice occurs and less than that at which substantial irregularities in cross-sectional area or shape occurs; and 5) permitting the ejected mixture to expand unrestrained in at least one dimension to produce an elongated thermoplastic cellular body.
The present foam offers excellent cushioning properties and resiliency. The present foams are suitable for cushion packaging since the foams have adequate impact absorption properties and resilience.
The foam products mitigate impact during multiple drops.
The foams absorb dynamic impacts surprisingly well, WO 94/13460 ~ ~ ~ ~ PCTILTS92/10934 particularly given they are open cell. In addition, the open cell foams can be used for sound absorption. The foams can be used for thermal insulation as well.
The present foam has satisfactory dimensional ' stability even though it is expanded with fast permeating blowing agents. Preferred foams recover ? $0 percent of initial volume within a month with initial volume being measured within 30 seconds after extrusion.
The following are examples of the present invention, and are not to be construed as limiting.
Unless otherwise indicated, all percentages, parts, or proportions are by weight.
Example 1 Open-cell propylene polymer foams of the present invention were prepared according to the present invention. Desirable foaming temperature ranges for making open-cell foams were determined.
The equipment employed was a 1 inch (in) (2.5 centimeters (cm)) screw type extruder having additional zones of mixing and cooling at the end of usual sequential zones of feeding, metering, and mixing.
An opening for blowing agent is provided on the extruder barrel between the metering and mixing zones. At the end of the cooling zone, there is attached a die orifice having an opening of rectangular shape. The height of the opening, hereinafter call die gap, is adjustable while its width is fixed at 0.115 in (3.68 millimeters (mm)).
A granular high melt strength (HMS) ' .
polypropylene resin having 0.54 melt flow rate (per ASTM

21~~0~8 ~O 94/13460 PCT/US92/10934 D-1238 Condition L) and tan delta of 0.92 was blended with a small amount, 0.1 pph (parts per hundred by weight per 100 parts polymer by weight) of Irganox 1010 brand antioxidant (from Ciba-Geigy Corp.), and fed into the extruder at a uniform rate of approximately 4 pounds per hour (lbs/hr) (1.$ kilo rams g per hour (kg/hr)). The temperatures maintained in the extruder zones were 175°C
a_t feeding zone, 210°C at melting zone, 230°C at metering zone, and 230°C at mixing zone. A 60/40 by mole (or 70/30 by weight) mixture of HCFC-1~42b and EtCl was prepared in a weigh tank, and injected under pressure into the mixing zone at a uniform rate of 0.76 lbs/hr (0.34 kg/hr). The rate amounted to 0.22 pound-moles per one hundred pounds of polymer (abbreviated as mph hereinafter). The level of 0.22 mph corresponds to 0.22 kph (kilogram-moles per hundred kilograms). The die gap was set at 0.012 in (0.30 mm). The temperature of the homogeneous polymer/blowing agent mixture about to undergo foam expansion (called the foaming temperature hereinafter) was gradually reduced by adjusting the temperature of the cooling zone. At each foaming temperature, a foam specimen was obtained. After about a week, each specimen was subjected to certain physical property tests.
Good-quality foams were made at a wide range of foaming temperatures. Table 1 relates the foam density and open cell content with the foaming temperature. At a foaming temperature higher than 161°C, the foam collapsed totally or partially. At 164°C, a temperature region where a stable, open cell foam could be made was approached. At a foaming temperature range from 161°C
to 155°C, foams having 60-70 percent open cells were produced. As the temperature was dropped further, both _ 13_ WO 94113460 ~ ~ ~ ~ PCT/US92/10934 the open cell content and the foam density decreased until the temperature reaches 150°C. Below 150°C, the foams were essentially close-cell, and the foam density leveled off. At a foaming temperature of 113°C, indications of freezing of the melt in the cooling zone were observed in the form of lumps in the foam body and variations in the shape of the foam strand. As seen in Table 1, the temperature window (OTf) for the closed-cell foam was approximately 1 ~+~°C-150°C ( ~T f = 7°C ) f or this polymer/blowing agent system. That for the partially open-cell foam was 151°C-163°C (~Tf = 13°C).
If the threshold temperature for a closed-cell foam is defined as Tf,max~ the operable foaming temperature for the partially open-cell foam was in the range between (Tf,max + 1) and (Tf,max + 13). The range will vary according to polymer/blowing agent systems. For this system, the optimum foaming temperature for a elosed-cell foam was approximately 117°C (middle point of the range for closed-cell foams). This example showed that a substantially open-cell foam can be extruded from a polypropylene/organie blowing agent system by a proper control of foam density, cell size and foaming temperature.

-1~!-~'VO 94/13460 PCT/US92/10934 Foaming Foam DensityCell Size D
(Pct (kg/m3)2(mm)3 (pcPmm)4 CPen CelS
(percent) 164 --Foam collapsed y_ partiall 163 1.66 (26.6) 0.95 1.58 69 162 1.63 (26.1 0.95 1.55 70 ) 161 1.59 (25.4) 0.95 1.51 67 160 1.51 (24.2) 1.08 1.63 62 159 1.55 (24.8) 1.47 2.28 68 158 1.65 (26.4) 1.47 2.43 66 157 1.62 (25.9) 1.47 2.38 71 156 1.48 (23.7) 1.80 2.66 69 ~ 155 1.49 (23.8) 1.80 2.68 69 154 1.44 (23.0) 1.80 2.59 45 153 1.35 (21.6) 1.80 2.43 31 152 1.37 (21.9) 1.35 1.85 20 151 1.35 (21.6) 1.47 1.98 21 150* 1.27 (20.3) 1.47 1.87 g 149* 1.27 (20.3) 2.03 2.58 6 148* 1.29 (20.6) 2.03 2.62 6 147* 1.34 (21.4) 1.62 2.17 5 146* 1.31 (21.0) 1.62 2.12 145* 1.31 (21.0) 1.47 1.93 5 144* 1.32 (21.1 1.47 1.94 0 ) 143* 1.34 (21.4) 1.35 1.81 4 TtVOtwithm the scope of this invention.
3 0 1 Temperature in degrees Celcius of the polymer/blowing agent mixture about to undergo foam expansion 2 Density of foam body in pounds per cubic foot (kilograms per cubic meter) measured in about 9 days after foam expansion Cell size in millimeters determined per ASTM D3576 9 The product of foam density and cell size 5 Open cell content in percentage determined per ASTM D2856-A

WO 94/13460 ~ ~ ~ PCTIUS92/10934 Example 2 Open-cell propylene polymer foams of the present invention were prepared according to the present invention. Desirable blowing agent levels for making open-cell foams were determined.
The apparatus, polymer and blowing agent of Example 1 were employed.
The effect of blowing agent level on foamability of the polypropylene resin was determined.
The foaming temperature was to be kept constant at 118°C, but was raised to 151°C for 0.13 mph (0.13 kph) blowing agent level to prevent the polymer melt from freezing. The process and property data are represented in Table 2. At 148°C foaming temperature, where a blowing agent level of 0.22 mph (0.22 kph) provided a closed cell as seen in Example 1, 0.19 mph (0.19 kph) blowing agent also provided a substantially closed-cell foam. Open cell content increased as the level of the blowing agent decreased--36 percent at 0.16 mph (0.16 kph) and 69 percent at 0.13 mph (0.13 kph). At 0.13 mph blowing agent level, a small amount of talcum powder was added to reduce the cell size and the foaming temperature was increased.

~~~a~~g O 94/134b0 PCT/US92l10934 Blowing Talc Foaming Foam Open T

est Agent DensityCell pfD
Level Temp Size No. Level . (pc (mm)5 (pcf Cell .> f) mm)s (pph)-(C)3 (mph)1 (kg/m3)4 (Percent) I1.1 0.19 -- 148 1.37 1.62 2.22 2 *

(21.9) 11.2 0.16 -- 148 1.61 2.03 3.27 36 (25.8) 11.3 0.13 0.03 151 2.01 1.01 2.03 69 (21.2) ..u...aaa c~uau~sac ua uaaaa auvcamou Pound moles of blowing agent mixed in per one hundred pounds of polymer (corresponding to kph) Parts of talcum powder mixed in per one hundred parts of polymer by weight Temperature in degrees Celsius of the polymerlblowing agent mixture about to undergo foam expansion Density of foam body in pounds per cubic foot (kilograms per cubic meter) measured in 9 days after foam expansion Cell size in millimeters determined per ASTM D3576 The product of foam density and cell size Open cell content in percentage determined per ASTM D2856-A
Example 3 Open cell foams of the present invention were prepared according to the present invention. The foams were prepared with a propylene copolymer.
The apparatus as in Example 1 was employed. A
2/98 (by weight) ethylene/propylene random copolymer having 0.39 melt flow rate (ASTM D-1238 Condition L) and 1.09 tan delta was foamed by the procedure of Example 1 with the blowing agent of Example 1. As in Examples 1 and 2, 0.1 pph antioxidant (Irganox 1010) was employed.
The temperatures maintained at the extruder zones were 160°C at feeding zone, 180°C at melting zone, 200°C at _ 17_ WO 94/13460 ~ ~ PCT/US92/10934 metering zone and 230°C at mixing zone. Foams were prepared over both a foaming temperature range and a blowing agent level range. As the foaming temperature was decreased, the die gap was slightly increased from 0.012 in (0.30 mm) to 0.017 in (0.13 mm) to achieve the desired foam cross-section without prefoaming.
Low density, open-cell foams were made using the copolymer resin at a relatively wide foaming temperature range. As seen in Table 3, making a elosed-cell foam with the copolymer resin was difficult as indicated by the narrow range of foaming temperature (139°C-141°C) for low open-cell content. In contrast, low density, open-cell foams are easily achieved from this resin for the temperature range of 112°C-117°C. The foaming temperature 1~4~4°C-145°C yielded open-cell foams with optimal X40-50 percent open cell content and the lowest foam densities.

~ 94/13460 ~ PCTIUS92110934 Blowing Talc Foamin Foam g Test Agent LevelTem densityCell pfp open p Size No. Level (pp . (pcf) (mm)5 (pcf Cell ) (~) mm)s h 3 (mph)' (kg/m3)a (Percent) 111.1 0.22 -- 151 3.34 0.65 2.17 40 (53.4) " 150 2.74 0.85 2.33 35 (43.8) " 149 2.02 0.81 1.64 86 (32.3) " 148 1.80 0.95 1.71 80 (28.8) " 147 1.53 0.90 1.38 45 (24.5) " 146 1.43 0.90 1.29 61 (22.9) " 145 1.38 1.01 1.39 43 (22.1 ) " 144 1.37 1.10 1.38 47 (21.9) * " 143 1.40 1.01 1.41 15 (22.4) " 142 1.44 0.95 1.37 23 (23.0) * " 141 1.43 0.95 1.36 12 (22.9) * " 140 1.42 1.01 1.43 3 (22.7) * " 139 1.40 0.85 1.19 12 (22.4) 111.2 0.19 -- 142 1.55 0.95 1.47 83 (24.8) 111.3 0.19 0.03 141 1.55 0.85 1.32 47 (24.8) wwr..._ -Pound moles of blowing agent mixed in per one hundred pounds of polymer (corresponding to kph) Parts of talcum powder mixed in per one hundred parts of polymer by weight Temperature in degrees Celsius ofthe polymer/blowing agent mixture about to undergo foam expansion Density offoam body in pounds per cubic foot (kilograms per cubic meter) measured in 9 days after foam expansion Cell size in millimeters determined per ASTM D3576 The product of foam density and cell size Open cell content in percentage determined per ASTM D2856-A
- Test No. IIL1 constituted 13 foam specimens made with a constant blowing agent level and different foaming temperatures WO 94113460 ~ ~ PCTIUS92/10934 Example ~4 Open cell foams of the present invention were prepared according to the present invention. The foams were prepared using an accumulating extrusion system ' (AES).
The apparatus is as in Examples 1 through 3 except the die is replaced with the AES. The AES
consisted of a jacketed 300 cubic centimeter capacity pressure vessel, nitrogen pressurizing system, and a gap-adjustable 0.25 in (0.64 cm) width die orifice. The pressure vessel, the transfer lines, and the die were maintained at or slightly above the temperature of the foamable melt so that the material will neither acquire excessive heat nor become frozen off. After the desired foaming condition was established, the melt was accumulated in the vessel under nitrogen back pressure of about 700 pounds per square inch gauge (psig) 0 830 kilopaseals gauge (kPag)). After a prescribed amount of the melt was accumulated, nitrogen gas (regulated to 1300 psig (8960 kPag)) was introduced to the top of the vessel and the foamable melt was discharged out of the die orifice to expand.
Three 2/98 weight ratio ethylene/propylene copolymers having different melt flow rates were evaluated. One copolymer is as in Example 3. The tan delta values of the resins were 1.11 for the 0.26 MFR
resin, 0.87 for the 0.57 MFR resin and 1.09 for the 0.39 MFR resin. As in Examples 1 through 3, a 60/40 by mole mixture of HCFC-142b/EtCl was used as the blowing agent.
The data was summarized in Table ~4. All three resins provided good-quality foams having large cross-sections of 16-18 square centimeters (cm2), small cell size, and ~O 94/13460 PCT/US92110934 low densities. The operating temperature conditions were such that the open-cell contents varied widely from resin to resin. The 0.39 MFR resin provided almost fully open-cell foam at 110°C, while the 0.26 MFR
provided one having only 1 ~+ percent open cells at 1 X47°C.
A foam having an intermediate open cell content (27 percent) was accomplished from the 0.57 MFR resin at 145°C. Understandably, open cell contents of these foams may be altered by choosing a different set of operating conditions (temperature, cell size, and density).

g T i Blowin Talc FoamingFoam Open est Res Agent DensityCeIISizepfD
n T
p No. MFRI Level (pph~~~~) (pcf) (mm)6 (pcf Cell ' mm)7 (mph) i (kg/m3)5 (percent) IV.1 0.26 0.19 -- 147 1.18 0.58 0.68 14 *

2 ( 18.88) IV.2 0.57 0.18 -- 145 1.20 0.58 0.70 27 ( 19.20) IV.3 0.39 0.19 0.02 140 1.37 0.51 0.70 92 (21.92) 1~ V6 81a GanLUjILC Ul LiLlFi LL1V GILL1UI7 2 5 i Melt flow rate in decigrams per minute of 2/98 ethylene/propylene copolymer used; determined per ASTM D1238 at Condition L
Pound moles of blowing agent mixed in per one hundred pounds of polymer (corresponding to kph) Parts of talcum powder mixed in per one hundred parts of polymer by weight Temperature in degrees Celsius of the polymer/blowing agent mixture about to undergo foam expansion Density of foam body in pounds per cubic foot (kilograms per cubic meter) measured in 9 days after 3 ~ foam expansion Cell size in millimeters determined per ASTM D3576 The product of foam density and cell size s Open cell content in percentage determined per ASTM D2856-A

WO 94/13460 ~ ~ ~ PCT/CTS92/10934 Example 5 Open cell foams of the present invention were prepared according to the present invention. The foams were prepared with a high melt strength (HMS) ' polypropylene homopolymer and several different blowing agents.
This apparatus and operating procedure were substantially the same as in Example 1. An HMS
polypropylene homopolymer having melt flow rate (MFR, the MFR was determined per ASTM D1238 at Condition L
unless otherwise specified herein after) and tan s of 1.09 was expanded with several different blowing agents.
For mixed blowing agents, constituent blowing agents were remixed p prior to injection into the extruder. As shown in Table 5, a small amount of talcum powder was incorporated in some tests for reduction of cell size.
In tests where HFC-134a is used as a blowing agent, a small amount of glycerol monostearate (GMS) was incorporated to enlarge the cell size. GMS, in concentrate form, and tale were preblended with the polypropylene granules and fed into the extruder at a uniform rate of ~4 pounds per hour (1.81 kgs/hr). The temperature maintained in the extruder zones were 150°C
at the feeding zone, 200°C at the melting zones, 220°C at metering zone, and 230°C at mixing zone.
The cooling zone temperature was maintained to uniformly cool the gel (melt mixture of polymer and blowing agent) down to about 150°C-151°C. The die opening was adjusted for each gel to yield foam strands free of prefoaming. Foam dimensional stability was measured with two specimens of about 5 inch ,(12.7 em) in length. As set forth in Table 5, all the single or 2~5Q~~.8 ~O 94/13460 PCT/US92/10934 mixed blowing agents provided good-quality, low-density foams having 2~4 percent or greater open cells at the foaming temperature. All foams meet the foamability criterion, prD ~ X1.28 pcf~mm (68.5 kg/m3~mm). With the relatively high open cell contents, all foams exhibit excellent dimensional stability.

_23_ WO 94/13460 ~ ~ ~ PCT/US92/10934 o ~ o z ~ o ~

o . .
o o o , c '''' -c 00Q1 Ctl0 N 01 O N 00~ p1 ' N Ct N 00 inN M 1G N tD 00 Q

H

a~
_o~ L

I~O u100 01~- CtM 1~M tG
lDC1 ~ 00 - N N O 01M ~ m 0 0 0 0 0 0 O Cta v o Q

O
to 00I~ O !f1O N C1 N M

it1~ M ~1 tC00 O

E O O O O O O O O O N
V

V o x .

.rA

M 1~ u'fM 1~1~ 1~00 01M 00R y v N 00 M N O O N M .-t0 N

N N N M M M M N N M

D

~ C~f~ i~C~ N N ~t I~~t tn ~

p v M ~ M C1C1 O .- IntD O a> ' ~t Q- N N N
L

, o _. . . ._. _ . ,..

00 ~

N N ~ tf1tf1 v O O O o bo O O O O O O ,,, _ 00 t4 a_-~ Q C "O a O

Q N v v v N N N

r o o + .R
DD

.~

L 4 d gy ~
~

~ N N N N N N LON tDC1 C1~ f/~
- - .
p ~

N N N N N N r . ~ ~ ~ s c a~ ,~
p O O O O O O O O O 0 0 ~ ~et~, ~., ~.ty o N, o a E, cu y ~ ~ ~ V1 O O O O O O b p a ~ ~ - d .~ ~ ~ ~ ~ ~ V~C
~ ~
~ L

rC '~ a ~
' a N

lWD lOlC lW C ~ ~l ~ N
N v ,D

t, ~ ~. fA

~ Q ~
O
~ ~ ~
~
~

~1 M . ~
b ~, ., ~
~
' RS
t ~ ~
?G
L
~ r V ~ ~ .
a t~ e~ m ~ ~ m ~- N ~ ~,~ C ~ N \t ~ .~ .n o o ~ b B ~ ~ ~ o V ~t to N V n E o .~
p ~ ~ ~ ~

N M ~ M = ~ Z .
~
::

"

V ~ ~ U V V m V ~ 3 ti ..o~
m~
o.
~4 ~
E
o V ~ V titi n M ~ n N ...~ ~ ~
o aj a aW.
. w = Z Z V ~ Z ~ ~ ~;~ o m~ o o.~

V Z V = U II L ,D i1 o y N
~ w ~ .
d~ ~a c V~ '~ ~m ~ cs, ~ .

U o , V = = ~
A
o H

c~p . CSC
.
AU
O~

N ~-N M ~ V1~C 1~00 a1~ _ .H N M V' ~ t0 t~ 00 Oo ~
O

O U1 p ~(1 N N

O 94/13460 ~ PCT/US92110934 Example 6 Open cell foams of the present invention were prepared according to the present invention. Low density, large cross-section open cell foam planks were prepared using a multi-orifice die and a forming plate assembly.
The apparatus was substantially the same as in Example 1 except for a different extruder and die. The extruder was a 1 1/2 inch (3.8 em) single screw type.
The die was a multi-orifice die with 0.030 inch (0.76 mm) diameter orifices arranged in rows and columns in a equilateral triangular pattern with 0.14 inch (3.7 mm) spacing between holes. Seventy-two holes (8 rows and 9 columns) were open. A forming plate assembly was attached at the die face. The forming plate assembly consisted of two horizontal forming plates and two guide shoes designed to guide the edges of the foam. The forming plates were made of carbon graphite, and the clearance between the two plates was adjustable by moving the plates vertically. The side shoes, angled X45 degree outward and lined with Teflon (trademark of E.I. DuPont de Nemours & Com) sheet, could be moved in and out.
A HMS 2/98 ethylene/propylene random copolymer having a melt flow rate of 0.5 and tan S of 0.96 was em to ed. The p y granular resin was mixed with 0.1 pph talcum powder for cell size control and 0.2 pph antioxidants. The antioxidants consisted of 50 percent IRGANOX 1010 brand hindered phenol-type (Ceba-Geigy Corp.) and 50 percent ULTRANOX 626 brand (Bo~rg-Warner Chemical, Inc.) phosphite-type. The antioxidants were WO 94113460 ~ ~ ~ ~ ~ ~ PCTIUS92/10934 made into a concentrate form in the base resin. The solid mixture was fed into the extruder at a uniform rate of approximately 10 lbs/hr (~4.5 kg/hr). The temperatures maintained at the extruder zones were 185°C
at feeding zone, 200°C at melting zone, 230°C at metering zone, and 200°C at mixing zone. A 60/40 by mole mixture of HFC-152a and ethyl chloride was injected under pressure into the mixing zone at a uniform rate of 1.37 lbs/hr (0.62 kgs/hr) which amounts to approximately 0.21 mph. The homogenized mixture of polymer and blowing agent was cooled down to approximately 157°C at the die to produce stable foam strands.
After an unfoamed sample was taken, the forming plates were applied to both sides of foam surfaces and the side shoes were moved in to guide the foam body at the edges. In order to overcome the drag created by the plates, the foam body must be gently pulled away. As seen in Table 6, forming had a significant effect on the foam quality, density and cross-sectional size. The unformed foam body, was a collection of loosely coalesced cylindrical strands, with channels among the strands, relatively high foam density, small cross-section and rough surfaces reflecting the contour of the ' cylinders. Forming made the strands enlarged, deformed to hexagonal honey comb shapes, and compacted with no voids thereby providing an excellent quality foam having lower density, larger cross-sectional size and smooth skin. With its high open cell content, the foam was strong upon compression and recovered readily after compression.

~I~(~(~~8 ~i'0 94113460 PCTlUS92110934 TestFormingFoam Cell Strand D Open Density Size Thi Wid Pf k hs s No. Platen l 3 (mm)a Dia.s . t ~ Cell pcf kcm c (pcf (percent)9 mm) 6.1 no 1.9831.7 0.36 3.1 2.4 3.3 0.71 71 6.2 yes 1.4022.4 0.54 6.7 3.8 6.0 0.76 66 no = free foaming without forming plates applied; yes = forming plates applied Density of foam body in pounds per cubic Foot aged for 14 days or longer after foam expansion Density of foam body in kilograms per cubic meter measured in 14 days after foam expansion Cell size in millimeters determined per ASTM D3576 Diameter of foam body in centimeters 1 0 s Thickness offoam body in centimeters Width of foam body in centimeters s The product of foam density and cell size Open cell content in percentage determined per ASTM D2856-A
Example 7 This example illustrates that forming leads to an open-cell polypropylene foam having desired well-balaneed strength distribution, resiliency and dynamic cushioning properties.
The apparatus was a 1-3/~I inch (t4.~4 em) screw type extruder having substantially the same configuration as the one of Example 6. The apparatus employed the multi-orifice die of Example 6. One hundred fifty-four holes (11 rows and 13 columns) were open at the die. The forming plate assembly was as in 3p Example 6.
The polypropylene resin of Example 6 was expanded with a 60/40 by mole mixture of HCFC-152b/EtCl, and then formed. The antioxidant package was as in Example 6. Talcum powder was employed at 0.5 pph. The solids were fed into the extruder at a uniform rate of _27_ WO 94113460 ~ ~ ~ PCT/US92/10934 approximately 25 lbs/hr (11.4 kg/hr). The temperatures maintained at the extruder zones were 175°C at the feeding zone, 200°C at melting zone, 230°C at metering zone, and 200°C at mixing zone. The premixed blowing agent was injected under pressure into the mixing zone at a rate of 4.1 lbs/hr (1.9 kg/hr), which amounts to 16.1 parts per hundred parts of polymer or approximately 0.19 mph.
The gel of melt polymer and blowing agent was cooled down to approximately 152°C to produce stable foam stands. The foam strands had fine cell size and approximately 3.7 mm in diameter loosely sticking to each other. The density of the foam strands was 32 kg/m3, and the cell size was 0.43 mm. The foam cross-section was small, and the foam surface was rough.
After an unformed sample was taken, the forming plates were closed together to give a drag on the foam, then the plates were opened to provide a large cross-section.
The side shoes were pushed in to guide the foam at the edges. The foam body was gently pulled away to overcome the drag created by the forming plates. With forming, an excellent quality foam having a larger cross-sectional size with well coalesced strands was achieved.
The strands were deformed to form perfect honeycomb shapes, and the foam surfaces turned smooth with the surface strands flattened out. Other benefits of forming may be noted from Table 5, where the properties of the formed foam body are compared. The benefits include a 28 percent reduction in foam density, almost tripling of foam cross-sectional size, and more balanced , directional strength. Ordinarily, an extruded foam plank sees strength oriented toward the extrusion direction, but the applied loads are often applied in ~O 94/13460 PCT/US92/10934 the vertical direction in actual cushioning applications. Table 7A clearly indicates that forming can redistribute strength toward the transverse directions (vertical and horizontal directions).
The open-cell polypropylene foam was tested for cushion packaging applications. All foam specimens had 1.5 inch (3.8 em) thickness (which is the stress direction), and 2.5 inch X 3.0 inch (6.~1 em X 7.6 cm) load bearing area. The peak deceleration experienced by a weight dropped on the foam specimens from a 2~1 inch (61 em) height was measured. The performance of the open-cell polypropylene in mitigating impacts during both the first and multiple drops indicated that its cushioning properties were adequate for most applications.

N

Z

N
y >31 u7 W N tI~

O
N

V tn O

n r~

C
C

Q ct t0 N
v M ~tp O
u , >
ar Y

V
m G.
2 t0 L

O

O O

L

v O O N

.

a O m m ~4 O

i1 H
v s E E a .o ,c m c ' ' c .

m n. ~ L o J ~ r- o~m ~

s M ~T~ d a, a Q f- a a m c .
a CO yr U

p =
.

b cc a~
E >

n t0 , i- M In~"" b ' N

Ca C

O
L v ~ ~ ~ ~ V

>s 4 N .p L In V1 p m ~

y a' :;
N y a on y G1 L .fl .

_ V ~ _ c .~ ~ ~ 2 >f~

O O ~ w ~ U1 d c1 V ' = v ~ ' ~ m V

..~
L d ~q W N ~ >a W
~

a a ~ a. ~ a ,'~ y '$ N

~ I~ ~ G V N d d V
V V ~
m 1 ~ i 7.
"'' .
' w m = E ~' .a ~ ~ C~

- _ n ~
M N ~ m ~ C C ' m ~
0 '~

~
w ' ~
C

N VU
~'O.~_~
'-~'' OU~
~

p G.'l~
L
.',_O, ~
W U.Ga ~ ~ .
-~ d ~

lfl ~ ~ 'O ~ ~ 'O LL

~ ~ ~ ~ .
C
, y "O
o o p '>? ~
~

u Q .a .. ..
.
p p O.Cl3~
C
~O
Cytp.

_ L
O
~
~

> m C
"' ~
~
~

.
c ~
C
~

O 4~ t~
~" C
J
4.
t O
L

C V", N .. ~
(~ 4~ '3 .~
O O ' ~
V ~ (p U

.
~" ~jd V ~ L G. V O V
"' C
.~ ~a' E
m O a d U
" II
a a ~ ,# -o a~ a~ p ~ A 4 c~ A H 3 H o ~
~

, p r' N ... N -. ~ .n o v- m c.

O Lfl O Lf1 In ~ ~- N N

2~~~~~.8 ~VO 94/13460 PCT/US92/10934 Pro Static PP Foams ert l p Stress= V E H
y Compressive Str. 80 57 86 (kPa) @25% Deflection Dynamic Cushioning (g) @ Static Stress (kPa) 1 st prop 1.7 74 70 82 ___ -5.8 46 51 48 7.6 48 56 46 9.4 S4 65 53 13.2 71 91 68 2-S Drop Average 1.7 86 71 8S

5.8 61 63 61 7.6 68 79 67 9.4 81 88 81 13.2 119 129 119 Compressive deflection at 2596 deflection in kilopascals determined per ASTM

Dynamic cushioning = peak deceleration in gs with a weight exerting the specified static stress during the first drop ( lEi Drop l and second through the fifth drops t2-5 Drop Average ) - Static stress exerted on the foam specimens in kilopascals s Properties measured in the vertical ( V ), extrusion ()r ), and horizontal (H 1 directions, respectively, for the polypropylene foam product Example 8 Open cell foams of the present invention were Prepared according to the present invention. The foams were prepared with a HMS propylene copolymer and subjected to forming.
The forming test of Example 7 was repeated with a HMS 2/98: ethylene/propylene copolymer having melt flow rate of 0.8 and tan value of 1.60. A sodium -3~-:. ' WO 94/134b0 PCT/US92/10934 bicarbonate/citric acid mixture-type (Hydrocerol CF-20 brand made by Boehringer Ingelheim KG, Germany) nucleator was employed as the cell size control agent.
Except for the cooling zone and die, the extruder zones ' were set at the same temperatures as in Example 7. In the tests of this example, there were employed mixed hydrocarbon blowing agents: a 60/40 by mole mixture of isobutane and normal pentane in Test 8.1 and a 70/30 by mole mixture of isobutane and normal butane in Test 8.2.
The polymer extrusion rate was maintained at 25 lbs/hr (11.3 kg/hr), and the blowing agent rate was adjusted so that its level would be 0.25 mph in both tests. A total of 156 holes (12 rows X 13 rows) and 143 holes (11 rows X 13 rows) were opened in Test 8.1 and 8.2, respectively. Good foams were made when the gel was cooled down to approximately 137°C and 140°C in Test 8.1 and 8.2, respectively. The forming plate assembly was applied to the foam strands coming out of the die.
Excellent quality foams were achieved in both tests.

~'O 94113460 PCT/US92110934 a z z >
.C
'~

, .-.

D M
'~
=

iu z M
Q
N

O
N

U ~ N

z w C
C

~DN

tDn ~U

Q >
y c~
0.

m G.~ p o v y ,, Q V
L

O O

.

G
c N

~
' n o r .
.

y d L

' c0 m '~ 'E

w C

,J~ 00O~ a a ~fM m m d d ..fir V
C ~.

fno ~
o ~ a L

H 00lG
E

E O O

L! E ~ ~ m Ca n m o c. a a .
c o ,o E c~-N ~ II c '.~o ~M ~C
a v -' A

N N ~ ~ ~ 8 ~ a rk w g ~

d c d c .n L' O V 'S a y m L V

(D ~ ~ M y C- ~ m 4 rm. ~'n ~ ~C ~

v L d ~ d O r.
Q a ~_ ~ m d ~ W a' as o a E n E

' ~
m w L ~~o~
NO~~
~U7 _ _ II LV C. .9C .p ...~.
y ~N V 3'' a R 00~O m (z., ~ ~ L a, V m ~n 1.

O O .
U U a ~~
o ~ 'o c ~ n , ~
.
.
C
C O y .d ~ E .~F.
~ 'B

L
m N m .C L E E

U
~
O
=
n x o E E
~ -~ ~ s N v ~

_ E~.-Ecinasc ~-eoo .

w v m .~ O N d U U 4' ao ' oT~
~
E
~' _ .
O ..
...
4o ~.
.
~ ~ o o ~
~ c , 3 ~ ~ .

.., ~ ~
' II
.
~ o v ' 'in x s ~ a c v m -a d ~

U U a -U y a - Vpm,AG7UH~H0=

o _ _ _ x C7 H ~ N ... cv ch v .n s r-Q s c .~0, ~z O lf1 O
N

. ~.

Example 9 Open cell foams of the present invention were prepared according to the present invention. The foams were prepared using a larger-scale apparatus with a multi-orifice die.
The apparatus having substantially the same configuration as in Example 1 except a 3 1/2 inch (8.9 em) screw type extruder and a different die. The die was a multi-orifice die having 2016 orifices of 0.011 inch (1.04 mm) diameter arranged in 18 rows and 112 columns in a equilateral triangular pattern with 0.25 inch (0.64 cm) distance between orifices. The operating procedure was substantially the same as in Example 1.
A HMS 2/98 ethylene/propylene random copolymer having a melt flow rate of 0.34 (ASTM D-1238 Condition L) was mixed with 0.05 pph talcum powder and 0.2 pph antioxidants. The antioxidants consisted of 50 percent by weight Irganox 1010 brand hindered phenol-type (Ciba-Geigy Corp.) and 50 percent by weight Ultranox 626 brand (Borg-Warner Chemical, Ine.) phosphite-type by weight.
The antioxidants had been pre-compounded into master batches in the base resin. The solid mixture was fed into the extruder at a uniform rate of approximately X100 lbs/hr (1$2 kg/hr). The temperatures maintained at the extruder zones were 130°C at feeding zone, 200°C at melting zone, 230°C at metering zone and 210°C at mixing zone. HCFC-142b was injected under pressure into the mixing zone at a rate of 79 lbs/hr (36 kg/m3), which amounts to 19.8 parts per hundred parts of polymer or approximately 0.20 mph (0.20 kph). When the homogeneous mixture of polymer and blowing agent was cooled down to approximately 154°C, a good foam having a fine cell size -3~+-~I~-~~~~
~O 94/13460 PCT/US92/10934 was achieved. The foam strands coalesced well together resulting in a foam plank with most of the interstices or channels filled. The foam cross-sectional size was approximately 2.~4 in X 23.$ in (6.1 cm X 60 em).
The foam exhibited excellent dimensional stability during aging suffering almost no change (less than 1 percent). Properties of the foam were determined in two weeks after extrusion. The foam had 1.48 pcf (23.7 kg/m3) density, 0.58 mm cell size, and 61 percent 1O open cells. The foam had a vertical compressive strength of approximately 7 psi (~18 kPa) at 25 percent deflection and, after 80 percent compressive deflection, recovered well to 95 percent of its original thickness within one hour and 96 percent of its original thickness within one day. The foam had a thermal conductivity of 0.295 B.t.u. /(hr) (ft2) (F°/in) (0.012 W/m.K°) . With its resiliency and low thermal conductivity, the polypropylene foam is not only suitable for cushion packaging but also for insulation applications.
Example 10 Open cell foams of the present invention were prepared according to the present invention. The foam was prepared in plank form with a HMS polypropylene homopolymer.
The foaming apparatus, the resin feedstock, and blowing agent were substantially the same as in Example 9 except a gap-adjustable slit die of 1 inch width was employed to produce a plank foam.
The polymer feedstock was mixed with.
antioxidant package of Example 9. Talc was not incorporated. The feedstoek was fed into the extruder WO 94113460 ~ ~ ~ ~ ~ PCTIUS92/10934 at a uniform rate of approximately 250 lbs/hr (114 kg/hr). The extruder zones were set at the same temperatures as in Example 5. HCFC-142b was injected under pressure into the mixing zone at a rate of 50 ' lbs/hr (23 kg/hr), which amount to 20 parts per hundred parts of polymer by weight or approximately 0.20 mph (0.20 kph). When the gel of melt polymer/blowing agent was uniformly cooled down to an optimum foaming temperature of 153°C, the die gap was adjusted to prepare a foam free of prefoaming. At a die gap of 0.135 inch (0.343 em), which was the threshold die opening for prefoaming, a good quality foam of 1.9 in X
~.2 in (~4.8 cm X 10.7 em) cross-section was achieved.
Like the coalesced strand plank of Example 9, the foam exhibited excellent dimensional stability during aging with almost no shrinkage (less than 1 percent). Properties of the foam were measured two weeks after extrusion. The foam had 1.18 pcf (1$.9 kg/m3) density, 1.49 mm cell size, and 8~+ percent open cells. The foam had a vertical compressive strength of 5.8 psi (~+0 kPa) at 25 percent deflection and, after 80 percent compression, recovered to 91 percent of its original thickness within one day.
While embodiments of the foam and the process of the present invention have been shown with regard to specific details, it will be appreciated that depending upon the manufacturing process and the manufacturer's desires, the present invention may be modified by various changes while still being fairly within the scope of the novel teachings and principles herein set forth.
_36_

Claims (10)

CLAIMS:
1. A process for making a dimensionally-stable extruded propylene polymer foam having an open-cell content of greater than 20 percent, comprising:

a) heating a propylene polymer material comprising greater than 50 percent by weight propylene monomeric units based upon the weight of the propylene polymer material to form a melt polymer material;

b) incorporating into the melt polymer material a blowing agent to form a foamable gel;

c) cooling the foamable gel to a foaming temperature; and d) extruding the foamable gel through a die from a region of higher pressure to a region of lower pressure to form the foam, the process being characterized in that the blowing agent contains greater than 85 weight percent by weight of one or more organic blowing agents based upon the total weight of the blowing agent.
2. The process of Claim 1, wherein the foam is from 30 to 70 percent open cell.
3. The process of Claim 1 or 2, wherein the blowing agent is 1-chloro-1, 1 difluoroethane.
4. The process of Claim 1 or 2, wherein the blowing agent is a mixture of 1-chloro-1,1-difluoroethane and ethyl chloride.
5. The process of Claim 1 or 2, wherein the blowing agent incorporated into the melt polymer material contains 95 weight percent or more of one or more organic blowing agents.
6. The process of Claim 1 or 2, wherein the blowing agent incorporated into the melt polymer material further contains one or more inorganic blowing agents.
7. The process of Claim 1 or 2, wherein the blowing agent comprises 1,1-difluoroethane.
8. The process of Claim 1 or 2, wherein the blowing agent comprises a mixture of 1,1-difluoroethane and ethyl chloride.
9. The process of Claim 1 or 2, wherein the blowing agent is selected from the group consisting of isobutane, n-butane, and n-pentane.
10. A dimensionally-stable, open-cell, propylene polymer foam obtainable by the process of Claim 1 or 2.
CA002150018A 1992-12-17 1992-12-17 Open cell polypropylene foam and process for making same Expired - Lifetime CA2150018C (en)