AU721221B2 AU38439/97A AU3843997A AU721221B2 AU 721221 B2 AU721221 B2 AU 721221B2 AU 38439/97 A AU38439/97 A AU 38439/97A AU 3843997 A AU3843997 A AU 3843997A AU 721221 B2 AU721221 B2 AU 721221B2
Authority
AU
Australia
Prior art keywords
reaction
bed
fluidizing
reactor
temperature
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Ceased
Application number
AU38439/97A
Other versions
AU3843997A (en
Inventor
Paul R. Kruesi
James M. Tranquilla
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
EMR Microwave Technology Corp
Original Assignee
EMR Microwave Technology Corp
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by EMR Microwave Technology Corp filed Critical EMR Microwave Technology Corp
Publication of AU3843997A publication Critical patent/AU3843997A/en
Application granted granted Critical
Publication of AU721221B2 publication Critical patent/AU721221B2/en
Anticipated expiration legal-status Critical
Ceased legal-status Critical Current

Links

Classifications

    • CCHEMISTRY; METALLURGY
    • C22METALLURGY; FERROUS OR NON-FERROUS ALLOYS; TREATMENT OF ALLOYS OR NON-FERROUS METALS
    • C22BPRODUCTION AND REFINING OF METALS; PRETREATMENT OF RAW MATERIALS
    • C22B1/00Preliminary treatment of ores or scrap
    • C22B1/02Roasting processes
    • CCHEMISTRY; METALLURGY
    • C22METALLURGY; FERROUS OR NON-FERROUS ALLOYS; TREATMENT OF ALLOYS OR NON-FERROUS METALS
    • C22BPRODUCTION AND REFINING OF METALS; PRETREATMENT OF RAW MATERIALS
    • C22B1/00Preliminary treatment of ores or scrap
    • C22B1/02Roasting processes
    • C22B1/10Roasting processes in fluidised form
    • CCHEMISTRY; METALLURGY
    • C22METALLURGY; FERROUS OR NON-FERROUS ALLOYS; TREATMENT OF ALLOYS OR NON-FERROUS METALS
    • C22BPRODUCTION AND REFINING OF METALS; PRETREATMENT OF RAW MATERIALS
    • C22B11/00Obtaining noble metals
    • C22B11/02Obtaining noble metals by dry processes
    • CCHEMISTRY; METALLURGY
    • C22METALLURGY; FERROUS OR NON-FERROUS ALLOYS; TREATMENT OF ALLOYS OR NON-FERROUS METALS
    • C22BPRODUCTION AND REFINING OF METALS; PRETREATMENT OF RAW MATERIALS
    • C22B15/00Obtaining copper
    • C22B15/0002Preliminary treatment
    • C22B15/001Preliminary treatment with modification of the copper constituent
    • C22B15/0013Preliminary treatment with modification of the copper constituent by roasting
    • C22B15/0015Oxidizing roasting
    • BPERFORMING OPERATIONS; TRANSPORTING
    • B01PHYSICAL OR CHEMICAL PROCESSES OR APPARATUS IN GENERAL
    • B01JCHEMICAL OR PHYSICAL PROCESSES, e.g. CATALYSIS OR COLLOID CHEMISTRY; THEIR RELEVANT APPARATUS
    • B01J2208/00Processes carried out in the presence of solid particles; Reactors therefor
    • B01J2208/00008Controlling the process
    • B01J2208/00017Controlling the temperature
    • B01J2208/00026Controlling or regulating the heat exchange system
    • B01J2208/00035Controlling or regulating the heat exchange system involving measured parameters
    • B01J2208/00044Temperature measurement

Landscapes

  • Engineering & Computer Science (AREA)
  • Chemical & Material Sciences (AREA)
  • Mechanical Engineering (AREA)
  • Manufacturing & Machinery (AREA)
  • Materials Engineering (AREA)
  • Metallurgy (AREA)
  • Organic Chemistry (AREA)
  • Geochemistry & Mineralogy (AREA)
  • Geology (AREA)
  • General Life Sciences & Earth Sciences (AREA)
  • Environmental & Geological Engineering (AREA)
  • Life Sciences & Earth Sciences (AREA)
  • Manufacture And Refinement Of Metals (AREA)
  • Physical Or Chemical Processes And Apparatus (AREA)

Description

WO 98/08989 PCT/CA97/00561 -1- TITLE OF THE INVENTION METHOD FOR MICROWAVE INDUCED OXIDATION OF SULPHIDIC ORE MATERIAL IN FLUIDIZED BED WITHOUT SULPHUR DIOXIDE EMISSIONS REFERENCE TO RELATED CASES This application is a continuation-in-part of U.S. Patent Application Serial No. 08/703,703 filed August 27, 1996, entitled "Method and Apparatus for Oxidation of Sulphidic Ores and Ore Concentrates Without the Production of Sulphur Dioxide Gas" by the same inventors herein.
FIELD OF INVENTION This invention relates to a microwave fluidized bed reactor which is used to oxidize pyritic ores by controlling microwave power density, oxygen concentration and fluidizing gas flow in such a way as to prevent oxidation of the sulphur into gaseous sulphur dioxide.
BACKGROUND OF THE INVENTION Many commercially important metals occur naturally in chemical composition with sulphur and iron, including gold and copper. These sulphidic compounds are difficult to process to a state where the important metals can be recovered.
Methods for separating metals from their sulphidic host minerals fall into two categories: Pyrometallurgical recovery and hydrometallurgical recovery.
Pyrometallurgical recovery involves heating the ore mass and in the process decomposing the sulphide through oxidation resulting in the formation of sulphur dioxide gas. Hydrometallurgical recovery on the other hand involves the dissolution WO 98/08989 PCT/CA97/00561 -2of the ore constituents in a liquid medium in which one or more chemical reactions can be initiated which will cause the important metals to form a new, recoverable compound. Pyrometallurgical recovery is unsatisfactory today because of the formation of sulphur dioxide gas in the so-called roaster oxidation reaction.
Accordingly, this technique has largely been abandoned due to legislation restricting sulphur dioxide emissions. Hydrometallurgical recovery is also an unsatisfactory process because metal recovery is hindered and, in many cases, rendered practically useless in the presence of sulphidic compounds.
Recent developments in this area include bio-oxidation where bacterial enzymes are used to oxidize sulphidic ores. However, this process is highly sensitive to variables such as temperature, sulphur concentration, and the presence of other minerals that may be toxic to the bacteria. Furthermore, the process is extremely expensive and relatively slow, rendering it commercially unviable in many situations.
Conventional pyrite roaster reactions are described by: FeS 2 FeS S (II) 4FeS 70, 2Fe 2 0 3 4SO, (III) S 02 SO In reaction pyrite (FeS 2 is decomposed into pyrrhotite (FeS) and elemental sulphur In the presence of oxygen and at sufficiently high temperature the associated reactions (II) and include the oxidation of pyrrhotite to form hematite and sulphur dioxide, and of sulphur to form sulphur dioxide. These reactions are highly exothermic, hence it is not possible in conventional roasting reactors to prevent the temperature from increasing to the point where SO 2 is produced. In fact, in conventional roaster operation, this exothermic energy is necessary to provide the reaction energy needed to cause to occur. This reaction, when augmented by steam and oxygen, may be used as a means of producing high quality SO 2 as a desired product, as disclosed by Jukkola in United States Patent No. 3,632,312.
An alternative reaction to (II) is: (IV) 2FeS 2 1.502 Fe 2 3 4S by which pyrite is oxidized directly into hematite and elemental sulphur. Table 1 and Figure 4 present a thermodynamic analysis of this reaction at various temperatures.
WO 98/08989 PCT/CA97/00561 -3- Tryer, for example, teaches this reaction (IV) in Australian Patent No. 9674.
However, Tryer states in his disclosure that it is necessary to maintain the operating temperature within the range 800 0 C 1000°C to promote the combination of a high concentration of SO 2 with ferrous sulphide to produce sulphur, a process which often requires the introduction of additional SO, to make up the necessary concentration.
An associated reaction, the combination of sulphur with hematite to form magnetite (Fe 3
O
4 and SO 2 is described by: 3Fe,0 3 S 2Fe 3 04 0.5SO 2 which is described in Table 2 and Figure 3 and which is favored only for temperatures above approximately 800 0 K (527 0
C).
Thus, in order for reaction (IV) to be favored and to avoid the entire roaster reaction the operating temperature must be maintained below approximately 1000*K (727 0 Further, in order to avoid the reaction the temperature must be maintained below approximately 800 0 K (527 0 C) The most strongly favored pyrite reaction is the one which produces hematite (Fe 2 0 3 and SO 2 shown as the lowermost curve in Figure 4 from data in Table 3. In order to avoid this reaction, oxygen must be restricted to allow the production of elemental sulphur (central curve in Figure Accordingly, to limit SO, production, the preferred operating temperature is below 527*C where the reaction products of pyrite and oxygen are restricted to hematite and sulphur as described in reaction (IV).
The ability to maintain the otherwise highly exothermic oxidation reaction temperature below 527 0 C requires separate control of: the oxygen supplied to the reaction; the power (energy) introduced into the material; and (3) the gas flow through the reaction environment (coolant). Control of the aforesaid factors can be achieved, in association with the present invention, using a fluidized bed reactor with power supplied by microwave energy, for treating pyritic mineral ore.
Fluidized bed reactors are presently widely used in many ore processing applications where strong interaction between a solid product and gas medium is required and the use of microwave energy to provide some or all of the required reaction energy has been disclosed in, for example, U.S. Patents Nos.
3,528,179; 4,126,945; 4,967,486; 4,511,362; 4,476,098; 5,382,412 and 5,051,456.
The use of a fluidized bed reactor with a microwave source of power provides the ability to control the oxygen supply to the material undergoing treatment (which governs the rate of reaction and hence reaction temperature) independently of the microwave power (which supplies the energy to initiate the chemical reaction and compensates for other energy losses). The use of microwave energy also provided the unique ability to selectively heat certain materials in the presence of less absorptive gangue materials as is the case with pyritic ores.
The exhaust stream from the reactor is depleted of oxygen as a consequence of the oxidation reaction with the fluidized bed and consists principally of nitrogen. It has been found that by diverting and preferably cooling the exhaust stream and reintroducing it into the reactor with the fluidizing stream that it is effective as a coolant and thus provides the final factor required to achieve the preferred chemical reaction to process pyrite minerals under temperature conditions that provide reaction products that are free of SO 2 emissions.
f SUMMARY OF THE INVENTION *ooo 20 Thus the invention comprises a method of oxidizing pyritic ores using a reaction vessel. The method comprises the steps of: fluidizing a bed of pyritic ore in said reactor using a fluidizing gas; heating said bed of ore with microwave energy to initiate an exothermic oxidation reaction in the bed; and using a temperature of reaction in said bed at which the preferred reaction 25 products are hematite and elemental sulphur.
The invention also comprises a method of oxidizing pyritic ores using a fluidizing bed reactor. The method comprises the steps of: heating a bed °of pyritic ore with microwave energy to initiate an exothermic oxidation reaction within the bed; controlling the inflow of oxygen to the reaction in the reaction chamber; and cooling the temperature of the reaction in said bed to a temperature at which the reaction products are hematite and elemental sulphur, while continuing to supply said bed with microwave energy S .to selectively heat the pyrite in the presence of 0 WO 98/08989 PCTCA9700561 magnetite and hematite.
The invention still further comprises a method for the oxidization of pyritic ores, without the production of SO 2 as a by product, using a fluidized bed reactor powered by microwave energy. The method comprises the steps of: (a) isolating the vent gases from the reactor when in operation; cooling the said vent gases; and re-introducing the vent gases into the fluidization gases in the reactor to cool the internal reaction temperature.
BRIEF DESCRIPTION OF THE DRAWINGS The following is a description by way of example of a preferred embodiment of the present invention, reference being made to the accompanying drawings in which: FIGURE 1 is a cross sectional view of a fluidized bed reactor of the present invention; FIGURE 2 is a graph showing thermodynamic stability data of Table 1; FIGURE 3 is a graph showing thermodynamic stability data of Table 2; and FIGURE 4 is a graph showing the Gibbs Free Energy for various pyrite reactions from data of Table 3.
While the invention will be described in conjunction with the illustrated embodiment, it will be understood that it is not intended to limit the invention to such embodiment. On the contrary, it is intended to cover all alternatives, modifications and equivalents as may be included within the spirit and scope of the invention as defined by the appended claims.
DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS In the drawings, similar features have been given similar reference numerals. As illustrated in Figure 1 a reactor vessel, such as a fluidized bed reactor WO 98/08989 PCT/CA97/00561 -6comprises a tubular waveguide resonator reaction chamber or cavity 12, bed fluidizer screen 14, and a pressure chamber 16. The reaction chamber 12 is connected to a microwave energy source via waveguide fittings 18 and 20 which may include a coupling iris (not shown) as well as a pressurized gas seal 22. The reaction chamber 12 has a material inlet valve 24, material exit valve 26, gas inlet valve 28 and a gas exhaust port 30. Exhaust port 30 is connected to pipe 40 which is in turn connected to particulate separator 42 (which may be a cyclonic separator), and a first control valve 44. Control valve 44 is connected by pipe 41 to heat exchanger 46 and second control valve 48, which is connected by pipe 43 to the gas inlet valve 28.
Pipe 40 has a gas exit port temperature monitor 50 and an SO 2 sensor 52.
Solid material to be processed, usually pyritic ore, is introduced through the inlet valve and is to be fluidized by gas 32 which is supplied from an external source through pipe 43 to control valve 48 and the gas inlet valve 28. The introduction of gas will cause the material which has been introduced through the inlet valve to form a fluidized bed 34 which is suspended through the adjustment of the gas pressure in the pressure chamber 16 and the bed fluidizer screen 14. The fluidized bed is then ready for treatment with microwave energy which is introduced into the reaction chamber from the top via the waveguide fittings. When the bed is in a fluidized state, the solid material is heated by the dielectric and resistive effects caused by interaction between the electromagnetic field and the solid material constituents.
The fluidizing gas will be continuously pumped through valve 28 and exhausted through port 30 during the treatment process. The exhaust stream will be passed through particulate separator 42 to clean the gas of particulate matter (either fines blown free from the fluidized bed or sulphur powder produced from the reaction). The stream will then pass through control valve 44 by which some or all of the exhaust stream, which will be depleted of 02 and consist primarily of N 2 can be recirculated back to the chamber after being passed through heat exchanger 46 and second control valve 48. Second control valve 48 allows the exhaust gas to be mixed with fresh air, or gases (if required), to provide the fluidizing stream and act as a coolant for the reaction chamber to achieve the preferred chemical reaction to process WO 98/08989 PCT/CA97/00561 -7pyrite minerals under temperature conditions that provide reaction products that are free of SO 2 emissions.
The region 36 above the suspended fluidized bed 34 is generally essentially free of solid material and consists primarily of fluidized gas and gaseous reaction products. The gas seal 22 permits the transmission of microwave energy into the reaction chamber 12 while isolating the atmosphere and contents of the chamber from the connecting waveguide attached via fittings 18 and Treatment of a pyritic ore, according to the present invention, will now be described in greater detail.
The pyritic ore is loaded into the reaction chamber 12 through valve 24. The ore is then fluidized into the bed 34 by pumping a fluidizing gas, which is generally just air, through valve 28. Next microwave energy is applied, via the waveguide fitting. The microwave energy raises the fluidized bed to the preferred operating temperature in the range of about 300°C 550°C, where as can be seen from the data of Table 1 and shown in Figure 2, pyrite is preferred over pyrrhotite.
Additionally, as can be seen in Table 2 and Figure 3, recombination of hematite and sulphur (reaction is not favoured at temperatures below 550'C. Once the temperature of the bed has been raised to about 300'C the sulphur-hematite reaction commences. If the temperature rises too quickly the N 2 in the vent gasses is not yet sufficient to restrict the amount of 02 and thus cool the reaction), N 2 can be introduced into the fluidizing stream via valve 48. The reaction can be monitored by checking the particulate separator 42, which will reveal the presence of sulphur, an indicator of the reaction, or by a temperature spike from temperature probe 50 since the initial pyrite reaction is exothermic.
In view of the fact that pyrite reaction is extremely exothermic, the temperature of the reaction chamber will continue to rise (in conventional reactors the running temperature is usually between 600'C and 750'C), causing the release of
SO
2 unless the reaction is cooled to favour reaction (IV).
First of all, the reaction can be cooled by reducing the input of microwave energy; although, as will be discussed below, it is preferable to maintain at least some input of microwave energy, in the range of 0.5kw. The second control -8of the reaction temperature is through the manipulation of the recirculating gases which, due to the reaction in the chamber, has been reduced to primarily N 2 If the r.action has not sufficiently reduced the 02 from the circulating gases, additional inert gasses can be introduced into the stream to control the amount of 02 in the reactor.
Additionally, the recirculating gases themselves can be cooled prior to reintroduction into the reaction chamber.
Pyrite can be selectively heated while in the presence of magnetite and hematite since it absorbs microwave energy more efficiently. Accordingly, it may be treated by the continued application of microwave energy during the exothermic reaction which is ongoing in the reaction chamber while at the same time the mass of the bed is being cooled by the recirculating gas stream.
Once the treatment process has been completed and the fluidized material appropriately heated or processed, it is ejected from the reactor through port 30 by increasing the fluidizing gas pressure. Any material which has fallen through screen 14 during loading and processing of the chamber is removed through valve 26.
Although described as preferably being tubular, the reaction chamber 12 can be of any appropriate dimension or geometry as dictated by the microwave field distribution. Additionally, while being described as an iris coupled resonator, the reaction chamber may operate as a terminated waveguide (iris fully open) in which case the absorptive action of the load material gives the reactor the characteristics of a travelling-wave applicator.
AMlENDED 'ET Ap, 4 7 I I r' TABLE 1 Gibbs Free Energies (kcal) with increasing temperature for the Pyrite Oxidation Reaction Temp K 298 400 500 600 700 800 900 1000 Temp C 25 127 227 327 427 527 627 727 FeS2 -38.26 -37.28 -36.06 -34.7 -33.22 -31.66 -30.01 -28.25 FeS -24.37 -24.43 -24.61 -24.83 -25.07 -25.27 -25.44 -25.53 2 FeS2 1.502 Fe203 4S -76.52 -74.55 -72.12 -69.4 -66.44 -63.32 -60.03 -56.51 -177.42 -170.78 -164.37 -158.09 -151.91 -145.83 -139.84 -133.91 Sum -100.9 -96.23 -92.25 -88.69 -85.47 -82.51 -79.81 -77.41 TABLE 2 Gibbs Free Energies (kcal) with increasing temperature for the Sulphur Hematite Reaction Temp K 298 400 500 600 700 800 900 1000 Temp °C 3 Fe203 2 Fe304 0.5 S02 -532.27 -512.33 -493.12 -474.26 -455.73 -437.5 -419.52 -401.74 -485.32 -468.64 -452.71 -437.14 -421.92 -407.12 -392.77 -378.55 -35.83 -35.97 -35.99 -35.95 -35.88 -35.78 -35.66 -35.51 Sum 11.12 7.72 4.42 1.2 -2.08 -5.41 -8.91 -12.32 0 .00
C
00 00 TABLE 3 Gibbs Free Energies (kcal) with increasing temperature for pyrite reactions Temp 0
K
298 400 500 600 700 800 900 1000 1100 1200 Temp 'C 25 127 227 327 427 527 627 727 827 927 FeS2 FeS S 2FeS2 1.5 02 Fe203 4S 2FeS2 5.5 02 Fe203 4502 13.89 12.85 11.46 9.87 8.16 6.39 4.58 2.72 0.81 -1.2 -100.9 -96.23 -92.25 -88.69 -85.46 -82.51 -79.81 -77.41 -75.32 -73.62 -387.73 -383.98 -380.16 -376.32 -372.52 -368.77 -365.11 -361.52 -357.98 -354.46 "comprises/comprising" when used in this specification is taken to specify the presence of stated features, integers, steps or components but does not preclude the presence or addition of one or more other features, integers, steps, components or groups thereof 9*
*S*
S

Claims (11)

1. A method of oxidizing pyritic ores using a fluidizing bed reactor which uses a fluidizing gas to fluidize a bed of pyritic ore, said method comprising the steps of: heating a bed of pyritic ore in the reaction chamber of said reactor using microwave energy to initiate a controlled, sub-autogenous exothermic oxidation reaction within the bed; controlling the inflow of oxygen to the reaction in the reaction chamber so as to avoid the reaction of oxygen with pyrite in order to limit production of SO 2 and using a temperature of reaction in said reactor within the range of about 300 0 C to 550 0 C at which temperature the reaction products are hematite and elemental sulphur.
2. A method according to claim 1 wherein step is a cooling step and S. comprises recirculating a portion of the outgoing fluidizing gases from the i reaction chamber back into the chamber. 0% 0 S o
3. A method according to claim 2, wherein N 2 or another inert gas is introduced into the recirculated fluidizing gas.
4. A method according to claim 2 wherein said recirculated gas is cooled by a heat exchanger.
5. A method according to claim 1 wherein step is a cooling step and comprises reducing the microwave energy that is supplied to the bed.
6. A method of oxidizing pyritic ores using a fluidizing bed reactor _-according to claim 1 wherein during step the microwave energy supply to itibed is continued to selectively heat the pyrite in the presence of magnetite* and ematite.
7. A method according to claim 2 further comprising the step of monitoring the temperature of the outgoing fluidizing gases.
8. A method according to claim 2 further comprising the step of monitoring the sulphur content of the outgoing fluidizing gases.
9. A method of oxidizing pyritic ores using a fluidizing bed reactor which uses a fluidizing gas to fluidize a bed of pyritic ore, said method comprising the steps of: heating a bed of pyritic ore in the reaction chamber of said reactor to a temperature in the range of 3000C to 5500C using microwave energy to initiate a controlled sub-autogenous exothermic oxidation reaction of pyritic ore into hematite and elemental sulphur within the bed; controlling the inflow of oxygen to the fluidized bed so as to avoid the reaction of oxygen with pyrite in order to limit production of SO 2 the "i inflow of oxygen being controlled to about stoichiometric quantities for the reaction: 2FeS 2 +3/202--Fe 2 O3+4S; and S: maintaining the temperature of reaction in said reactor within the range of about 3000C to 5500C at which temperature the products are hematite and elemental sulphur.
A method according to claim 9 wherein step comprises: removing a portion of the fluidizing gas from the reaction chamber of said reactor, cooling said portion of fluidizing gas via heat exchange and recirculating the cooled •portion of the fluidizing gas back into the reaction chamber.
11. A method according to claim 1 and as herein described with reference to Figure 1. '?Z I N A 13 DATED this 2 0 th day of April, 2000 EMR MICROWAVE TECHNOLOGY CORPORATION WATERMARK PATENT TRADEMARK ATTORNEYS 290 BURWOOD ROAD HAWTHORN VICTORIA .3122 AUSTRALIA P6445AUOO KJS/CLRISIG
AU38439/97A 1996-08-27 1997-08-08 Method for microwave induced oxidation of sulphidic ore material in fluidized bed without sulphur dioxide emissions Ceased AU721221B2 (en)

Applications Claiming Priority (5)

Application Number Priority Date Filing Date Title
US70370396A 1996-08-27 1996-08-27
US08/703703 1996-08-27
US89710397A 1997-07-18 1997-07-18
US08/897103 1997-07-18
PCT/CA1997/000561 WO1998008989A1 (en) 1996-08-27 1997-08-08 Method for microwave induced oxidation of sulphidic ore material in fluidized bed without sulphur dioxide emissions

Publications (2)

Publication Number Publication Date
AU3843997A AU3843997A (en) 1998-03-19
AU721221B2 true AU721221B2 (en) 2000-06-29

Family

ID=27107190

Family Applications (1)

Application Number Title Priority Date Filing Date
AU38439/97A Ceased AU721221B2 (en) 1996-08-27 1997-08-08 Method for microwave induced oxidation of sulphidic ore material in fluidized bed without sulphur dioxide emissions

Country Status (4)

Country Link
EP (1) EP0950122A1 (en)
AU (1) AU721221B2 (en)
CA (1) CA2263497A1 (en)
WO (1) WO1998008989A1 (en)

Families Citing this family (7)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
US5972302A (en) * 1996-08-27 1999-10-26 Emr Microwave Technology Corporation Method for the microwave induced oxidation of pyritic ores without the production of sulphur dioxide
AT408992B (en) * 2000-06-28 2002-04-25 Voest Alpine Ind Anlagen Process for the direct reduction of fine ore, and installation for carrying out the process
DE10260733B4 (en) 2002-12-23 2010-08-12 Outokumpu Oyj Process and plant for the heat treatment of iron oxide-containing solids
DE10260742A1 (en) * 2002-12-23 2004-07-08 Outokumpu Oyj Process and plant for the thermal treatment of granular solids in a fluidized bed
DE10260744A1 (en) * 2002-12-23 2004-07-01 Outokumpu Oyj Process and plant for the thermal treatment of granular solids
DE102010022400B4 (en) * 2010-06-01 2013-04-25 Outotec Oyj Process and plant for lowering the residual carbon content of ash
FR3136541A1 (en) * 2022-06-14 2023-12-15 Innovation & Development Company microwave and fluidized bed calcination furnace

Citations (3)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
US2209331A (en) * 1936-11-12 1940-07-30 Haglund Ture Robert Roasting process
US4678478A (en) * 1986-04-14 1987-07-07 Massachusetts Institute Of Technology Method for desulfurization of coal
US5123956A (en) * 1991-04-12 1992-06-23 Newmont Mining Corporation Process for treating ore having recoverable gold values and including arsenic-, carbon- and sulfur-containing components by roasting in an oxygen-enriched gaseous atmosphere

Family Cites Families (4)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
US4324582A (en) * 1980-06-11 1982-04-13 Kruesi Paul R Process for the recovery of copper from its ores
JPH0711594B2 (en) * 1987-05-21 1995-02-08 動力炉・核燃料開発事業団 Fluidized bed system
JP2766586B2 (en) * 1992-06-23 1998-06-18 大阪ガスエンジニアリング株式会社 Method and apparatus for roasting granular processed products
DE4329417C1 (en) * 1993-09-01 1994-08-18 Metallgesellschaft Ag Process for roasting refractory gold ores

Patent Citations (3)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
US2209331A (en) * 1936-11-12 1940-07-30 Haglund Ture Robert Roasting process
US4678478A (en) * 1986-04-14 1987-07-07 Massachusetts Institute Of Technology Method for desulfurization of coal
US5123956A (en) * 1991-04-12 1992-06-23 Newmont Mining Corporation Process for treating ore having recoverable gold values and including arsenic-, carbon- and sulfur-containing components by roasting in an oxygen-enriched gaseous atmosphere

Also Published As

Publication number Publication date
CA2263497A1 (en) 1998-03-05
EP0950122A1 (en) 1999-10-20
WO1998008989A1 (en) 1998-03-05
AU3843997A (en) 1998-03-19

Similar Documents

Publication Publication Date Title
US5972302A (en) Method for the microwave induced oxidation of pyritic ores without the production of sulphur dioxide
AU658146B2 (en) Preheating of iron ore feed, prior to reduction to iron carbide in a fluidised bed reactor
US5123956A (en) Process for treating ore having recoverable gold values and including arsenic-, carbon- and sulfur-containing components by roasting in an oxygen-enriched gaseous atmosphere
US20080069746A1 (en) Method and apparatus for microwave induced pyrolysis of arsenical ores and ore concentrates
AU721221B2 (en) Method for microwave induced oxidation of sulphidic ore material in fluidized bed without sulphur dioxide emissions
US20080118421A1 (en) Method and means for using microwave energy to oxidize sulfidic copper ore into a prescribed oxide-sulfate product
JPH06172835A (en) Method and device for reducing iron ore
WO2006048283A1 (en) Process and plant for producing titania slag from ilmenite
WO1989004379A1 (en) Microwave irradiation of mineral ores and concentrates
FI92223C (en) Process for the reduction of solid phase metal oxide-containing material
US3421884A (en) Method for carrying out gassolids reactions
WO2006097569A1 (en) Process and plant for the heat treatment of solids containing titanium
KR101016999B1 (en) Method for pre-heating iron agglomerates
US3034884A (en) Reduction roasting of iron ores
US1832731A (en) Treatment of iron ores
EP1370698B1 (en) Method for curing self-reducing agglomerates
RU2285048C2 (en) Method of production of iron-nickel alloys and nickel from oxide materials and plant for realization of this method
CA2566318A1 (en) A direct reduction process
Shu et al. Sintering and ferrite formation during high temperature roasting of sulfide concentrates
JPH0140881B2 (en)
US5248330A (en) Method of pyroprocessing mineral ore material
US4082542A (en) Copper precipitate agglomerization process
KR20020045617A (en) Method for direct reduction of materials containing iron oxide
US4465510A (en) Agglomeration of iron ores and concentrates
JPS58133327A (en) Manufacture of low sulfur content roasted ore

Legal Events

Date Code Title Description
FGA Letters patent sealed or granted (standard patent)
MK14 Patent ceased section 143(a) (annual fees not paid) or expired