AU612794B2 - Modified advanced epoxy resins - Google Patents

Modified advanced epoxy resins Download PDF

Info

Publication number
AU612794B2
AU612794B2 AU30382/89A AU3038288A AU612794B2 AU 612794 B2 AU612794 B2 AU 612794B2 AU 30382/89 A AU30382/89 A AU 30382/89A AU 3038288 A AU3038288 A AU 3038288A AU 612794 B2 AU612794 B2 AU 612794B2
Authority
AU
Australia
Prior art keywords
epoxy resin
document
component
formula
advanced
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Ceased
Application number
AU30382/89A
Inventor
John L. Massingill Jr.
Raul A. Pabon Jr.
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Dow Chemical Co
Original Assignee
Dow Chemical Co
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Priority claimed from US07/143,771 external-priority patent/US4835225A/en
Application filed by Dow Chemical Co filed Critical Dow Chemical Co
Application granted granted Critical
Publication of AU612794B2 publication Critical patent/AU612794B2/en
Anticipated expiration legal-status Critical
Ceased legal-status Critical Current

Description

£1FI1L.. rL-LIL.L-pt urmonae F1tzpatrick u~rira lratent counse Note N legahzacton or other wtness required,
I
i PCT OPI DATE 11/08/89 AOJP DATE 07/09/89 INTERNATIONAL APPLICA l APPLN. ID 30382 89 (51) International Patent Classification 4 C08G 59/02, 59/16 I (11) Internation PCT NUMBER PCT/US88/04678 al Publication Number: WO 89/ 06662 lalftlidliDMh 27 July 1989 (27.07.89) (21) International Application Number: PCT/US88/04678 (22) Internationl Filing Date: 28 December 1988 (28.12.88) Published With international search report.
(31) Priority Application Number: (32) Priority Date: (33) Priority Country: 143,771 13 January 1988 (13.01.88)
US
(71) Applicant: THE DOW CHEMICAL COMPANY [US/ US]; 2030 Dow Center Abbott Road, Midland, MI 48641-1967 (US).
(72)Inventors: MASSINGILL, John, Jr. 410 Forest Drive, Lake Jackson, TX 77566 PABON, Raul, Jr. 106 Mesquite, Lake Jackson, TX 77566 (US), (74) Agent: DAMOCLES, Nemia, The Dow Chemical Company, P.O. Box 1967, Midland, MI 48641-1967 (U (54)Title: MODIFIED ADVANCED EPOXY RESINS (57) Abstract Modified advanced epoxy resins are prepared by reacting an advanced epoxy resin prepared by reacting an epoxy resin having at least one aromatic ring, an average of more than one, but not more than about 2 vicinal epoxy groups per molecule and which contains at least one oxyalkylene or substituted oxyalkylene group per molecule: with a dihydric phenol; with a monoamine. Curable compositions comprising the modified advanced epoxy resin and cured products resulting from curing the curable compositions are also disclosed, i WO 89/06662 PCT/US8/04678 -1- MODIFIED ADVANCED EPOXY RESINS The present invention concerns advanced epoxy resins prepared from dihydric phenols and compounds having an average of more than one glycidyl ether group per molecule, at least one aromatic group per molecule and at least two alkoxy groups per molecule which advanced epoxy resins have been reacted with an amine.
Advanced aromatic epoxy res.ins are well known for their, extremely useful combination of properties 1 such as flexibility, adhesion, resistance to corrosion, and chemical and solvent resistance. Unfortunately, they also have some well known disadvantages sucln as sensitivity to ultraviolet light, relatively high viscosities, and limited formability. Advanced aliphatic epoxy resins are well known for their low viscosities and flexibility; however, they lack physical strength and are sensitive to water and chemicals. It would be desirable to have available advanced epoxy resins which have unique combinations of viscosity (low), and when cured with a suitable curing agent, good flexibility, strength and resistance to water and chemicals and solvents.
WO 89/06662 PCT/US88/04678 -2- One aspect of the present invention pertains to a modified advanced epoxy resin which results from reacting an advanced epoxy resin which results from reacting an epoxy resin composition comprising at least one epoxy resin having at least one aromatic ring, an average of more than one, but not more than two vicinal epoxy groups per molecule and which contains at least one oxyalkylene or substituted oxyalkylene group per molecule; and optionally at least one epoxy resin which has an average of more than one but not more than two vicinal epoxy groups per molecule and which is different from the epoxy resin of (a) 20 above; wherein components and are present in amounts such that from 5 to 100 equivalent percent of the epoxide groups are derived from component and from zero to 95 equivalent percent of the epoxide groups are derived from component with at least one compound having two aromatic hydroxyl groups per molecule; Swherein components and are employed in amounts which provide a ratio of aromatic hydroxyl groups per epoxy group of from 0.005:1 to 200:1; with a nitrogen-containing compound selected from primary monoamines; i I i r,- WO 89/06662 PCT/US88/0467?,,, -3secondary monoamines; tertiary monoamines; hydroxyl substituted primary, secondary or tertiary monoamines; or any combination of components or wherein components and are present in an amourt such that the ratio of amine groups contained in component to epoxy groups contained in component is from 0.1:1 to 1.1:1.
Another aspect of the present invention pertains to a curable composition which comprises (I) the aforesaid reaction product of the advanced epoxy resin and nitrogen-containing compound and (II) a curing amount of a suitable curing agent for component The compositions of the present invention have, unique combinations of viscosity (low), and when cured with a suitable curing dgent, good flexibility, strength and resistance to water and chemicals and solvents.
The advanced epoxy resins employed in the present invention are prepared by reacting the epoxy resin or mixture of epoxy resins with the compound having two aromatic hydroxyl groups per molecule or mixture of such compounds at a temperature suitably from 25°C to 300°C, more suitably from 50°C to 2500C, most suitably from 50°C to 225°C for a time sufficient to complete the reaction, suitably from 1 to 8, more suitably from 1 to 6, most suitably from 1 to 4 hours.
The higher the temperature, the shorter the reaction time and the lower the temperature the longer the i i i I WO 89/06662 PCT/US88/04678 -4reaction time. The reaction is usually conducted in the presence of a catalyst and if desired, one or more solvents. The reactants are employed in amounts such that the ratio of phenolic hydroxyl groups to epoxide group is suitably from 0.005:1 to 200:1, more suitably from 0.5:1 to 5:1, most suitably from 0.5:1 to 1:1.
The epoxy resin which is advanced with the compound having two aromatic hydroxyl groups has suitably from 5 to 100, more suitably from 10 to 100, most suitably from 25 to 100 percent of the epoxy groups derived from an epoxy resin which contains oxyalkylene or substituted oxyalkylene groups and suitably from zero to 95, more suitably from zero to most suitably from 5 to 75 percent of the epoxy groups derived from an epoxy resin which is different from the aforementioned epoxy resin.
Suitable epoxy resins having at least one 2 aromatic ring, an average of more than one, but not more than about two glycidyl ether groups per molecule and which contain at least one oxyalkylene or substituted oxyalkylene group per molecule include those represented by the following formula I WO 89/06662 PCT/US88/04678 Formula I 0 0
H
2 C C- CH 2
CH
2 C -CH2 R
R
wherein each R is independently hydrogen or an alkyl group having from 1 to 4 carbon atoms, preferably hydrogen or methyl, most preferably hydrogen; Z is a divalent aromatic group represented by the following formulas II and III Formula II Formula III
(X)
4
(X)
4
(X)
4 (A)n wherein A is a divalent hydrocarbyl group having suitably from 1 to 12, more suitably from 1 to 6, most suitably from 1 to 3, carbon atoms, -802-, or each X is independently hydrogen, a hydrocarbyl or hydrocarbyloxy group having suitably from 1 to 12, more suitably from I to 6, most suitably from 1 to 3 carbon atoms, or a halogen, more suitably chlorine or bromine, most suitably }c bromine; n is zero or 1; each Z' is WO 89/06662 PCT/US88/04678 -6independently a group represented by the following formula IV Formula IV -CH-CH- R2 RI wherein each R1 and R2 are independently hydrogen or a hydrocarbyl or hydrocarbyloxy group having suitably from 1 to 12, more suitably from 1 to 6, most suitably from 1 to 3 carbon atoms or an -CH 2 -O-R3 group wherein R 3 is a hydrocarbyl group having suitably from 1 to 12, more suitably from 1 to 9, most suitably from 1 to 6 carbon atoms; and each m and m' independently has a value suitably from 1 to more suitably from 1 to 10, most suitably from 1 to The term hydrocarbyl as employed herein means any aliphatic, cycloaliphatic, aromatic, aryl substituted aliphatic or cycloaliphatic, or aliphatic or cycloaliphatic substituted aromatic groups. The aliphatic groups can be saturated or unsaturated.
Likewise, the term hydrocarbyloxy means a hydrocarbyl group having an oxygen linkage between it and the object to which it is attached.
Particularly suitable epoxy resins which have an average of more than one but not more than two vicinal epoxy groups and at least one aromatic ring per molecule and at least one oxyalkylene group or substituted oxyalkylene group per molecule include, for example, the glycidyl ethers of the reaction products of an aromatic compound having two aromatic hydroxyl groups per molecule or mixture of such i ,i i- WO 89/06662; PCT/US8804678 compounds and an alkylene or substituted alkylene oxide or monoglycidyl ether or any combination thereof.
Suitable compounds having two aromatic hydroxyl groups per molecule which can be employed herein include, for example, those represented by the following formulas V and VI Formula V
(X)
4 HO OH Formula VI (4 X)4 HO OH wherein A, X and n are as defined above.
Particularly suitable aromatic compounds having two aromatic hydroxyl groups per molecule include, for example, catechol, hydroquinone, resorcinol, biphenol, bisphenol A, biIphenol 1 bisphenol K, bisphenol S, and combinations thereof. Particularly suitable alkylene oxides include, for example, ethylene oxide, 1,2propylene oxide, 1,2-butylene oxide, 2,3-butylene oxide and combinations thereof. Particularly suitable substituted alkylene oxides include, for example, styrene oxide, t-butyl styrene oxide, isopropenyl benzene oxide and combinations thereof. Suitable monoglyoidyl ethers include, for example, glycidyl ethers of ethylenically unsaturated monocarboxylic acids, alkyl glycidyl ethers, aryl glycidyl ethers and combinations thereof. Particularly suitable T IC WO 89/06662 PCT/US88/04678 -8monoglycidyl ethers include, for example, phenyl glycidyl ether, butyl glycidyl ether, glycidyl acrylate, glycidyl methacrylate, dodecyl glycidyl ether and combinations thereof.
Suitable epoxy resins which have an average of more than one but not more than two vicinal epoxy groups per molecule and which are different from the aforementioned epoxy resins include, for example, those aromatic epoxy resins represented by the following formulas VII and VIII as well as those aliphatic epoxy resins represented by the following formula IX Formula VII 0 H2C -C-CH2
I
0
(X)
4 0Oi 0 CH2-.C-CH2 -6 1
(X)
4 0 0 0 CH 2 -C CH2 ni R Formula V III 0 H2C-~ C-CH 2 -0
I
CH2 0
MX
4 S(A)n
(X)
4 0 CH2-C -CH 2
I
m WO 89/06662 PCT/US88/04678 Formula IX o a 0 0
H
2 C C--CH 2 0 (-CH-CH0)m CH 2 C -CH2
R
RZ
R Rl R wherein A, R, RI, R2, X, m and n are as defined above and n' suitably has an average value from zero to more suitabl- from 0.01 to 0.5, most suitably from 0.03 to 0.15.
Particularly suitable as the other epoxy resins are those epoxy resins which have an average of more than one but not more than two vicinal epoxy groups and at least one aromatic ring per molecule which are free of oxyalkylene or substituted oxyalkylene gr6ups.
The term free of oxyalkylene or substituted oxyalkylene groups means that the epoxy resin is free of groups represented by the following formulas X and
XI
Formula X -CH-CH-0- I I
R
2 R1 3b Formula XI -0-CH-CH- R2 R1 10a wheein R 1and R 2are as defined above, and the term oxyalkylene or substituted oxyalkylene group is defined accordingly.
,S
t Or DI i i i WO 89/06662 PCT/US88/04678 -11- Mre particularly suitable epoxy resins which have an average of more than one but not more than two vicinal epoxy groups and at least one aromatic ring per molecule and which are free of oxyalkylene groups include, for example, the glycidyl ethers of catechol, resorlnol, hydroquinone, biphenol, bisphenol A, bisphenol F, bisphenol K, bisphenol S, and any combination thereof.
The epoxy resins which are prepared from compounds having aliphatic hydroxyl groups which are reacted with an epihalohydrin can be prepared by any of Sthe known methods for preparing aliphatic epoxy resins such as corducting the reaction in the presence of a Lewis acid such as, for example, stannic chloride, boron trifluoiide and combinations thereof; followed by dehydrohalogenation with a basic acting compound such as an alkali metal hydroxide. Most preferably, these epoxy resins are prepared by the method disclosed in GB 2,137,205A.
Suitable catalysts which can be employed to prepare the advanced epoxy resins include, for example, tertiary amines, phoaphines, ammonium compounds, phosphonium compounds and metal hydroxide.
Partioularly suitably catalysts include, ethyl triphenyl phosphonium chloride, ethyl triphenyl phosphonium bromide, ethyl triphenyl phospLonium iodide, ethyl triphenyl phosphonium acetate.acetic acid complex, tetrabutyl phosphonium chloride, tetrabutyl phosphonium bromi.e, tetrabutyl phosphonium iodide, tetrabutyl phosphonium acetate.acetic acid complex and combinations thereof. The catalyst is suitably Semployed in an amount which corresponds to from 0.0001 to 0.02, more suitably form 0.002 to 0.02, most WO 89/06662 PCT/US88/04678 -12suitably from 0.002 to 0.02, moles of catalyst per mole epoxy resin.
Suitable solvents whSch can be employed in the preparation of the advanced epoxy resins include, for example, alcohols, ketones, glycol ethers, aliphatic hydrocarbons, halogenated aliphatic hydrocarbons, aromatic hydrocarbons and combinations thereof.
Particularly suitable solvents include, for example, toluene, xylene, propylene glycol methyl ether, propylene glycol butyl ether, propylene glycol monotertiary butyl ether, ethylene glycol monobutyl ether (2-butoxyethanol) and combinations thereof. The solvent can be employed suitably in amounts of from zero to 50, more suitably from 3 to 30, most suitably from 3 to 20 percent by weight based upon combined weight of thif epoxy resin and the phenolic compound.
Suitable nitrogen-coptaining compounds which can be employed herein to react with the advanced epoxy resins include, for example, ammonia, primary monoamines, secondary monoamines and tertiary monoamines. Suitable primary monoamines include those aliphatic and aromatic primary monoamines having suitably from zero to 20, more suitably from 2 to most suitably from 2 to 7, carbon atoms. Suitable such primary monoamines include, for example, ammonia, ethyl amine, ethanol amine and combinations thereof.
Suitable secondary monoamines include those aliphatic and aromatic secondary monoamines having suitably from 2 to 20, more suitably from 2 to 1C, most suitably from 2 to 7, carbon atoms. Suitable such secondary monoamines include, for example, diethylamine, diethanolamine, methyl ethanolamine and combinations thereof. Suitable tertiary monoamines include those i i WO 89/06662 pcT/us8/04678 -13aliphatic and aromatic tertiary monoamines having suitably from 3 to 20, more suitably from 3 to 10, most suitably from 3 to 6 carbon atoms. Suitable such tertiary monoamines include, for example, methyl diethanolamine and combinations thereof.
Particularly suitable nitrogen-containing compounds which can be employed to modify the advanced epoxy resins to prepare the modified advanced epoxy resins of the present invention include the hydroxylcontaining monoamines such as, for example, dimethyl ethanolamine, methyl dimethanolamine, ethanolamine, methyl ethanolamine and combinations thereof.
The nitrogen-containing compound is employed in an amount which provides a ratio of amine groups contained iin the nitrogen-containing compound, component to epoxy groups contained in the advanced epoxy resin, component suitably from 0.1:1 to 1.1:1, more suitably from 0.1:1 to 1:1, most suitably from 0.15:1 to 1:1.
If desired, the modified advanced epoxy resins of the present invention can be further modified with a volatile acid to prepare a quaternary ammonium compound. Suitable such acids include, for example, any aliphatic monocarboxylic acid having suitably from 1 to 10, more suitably from 2 to 4, most suitably from 2 to 3 carbon atoms. Particularly suitable aliphatic monocarboxylic acids include, for example, acetic acid, propionic acid lactic acid and combinations thereof.
The acid can be employed in amounts which provides a ratio of acid equivalents per amine group suitably from WO 89/06662 PCT/US88/04678 -14- 0.8:1 to 1.3:1, more suitably from 0.9:1 to 1.1:1, most suitably from 0.95:1 to 1:1.
The modified advanced epoxy resins of the present invention can be cured with any suitable curing agent for epoxy resins including, for example, primary and secondary polyamines, carboxylic acids and anhydrides thereof, phenolic hydroxyl-containing compounds, guanidines, biguanides, urea-aldehyde resins, melamine-aldehyde resins, alkoxylated ureaaldehyde resins, alkoxylated melamine-aldehyde resins, phenol-aldehyde (resole) resins and combinations thereof. Particularly suitable curing agents include, for example, diethylenetriamine, Nadic methyl Sanhydride, phenol-formaldehyde (resole) resins, cresolformaldehyde (resole) resins, bisphenol A-formaldehyde (resole) resins, melamine-formaldehyde resins, methoxylated melamine-formaldehyde resins, ureaformaldehyde resins, methoxylated urea-formaldehyde resins and combinations thereof. The curing agents are employed in an amount which will effectively cure the composition containing the epoxy resin. These amounts will depend upon the particular epoxy resin and curing agent employed; however, suitable amounts include, for example, from 0.025 to 4, more suitably from 0.5 to 2, most suitably from 0.75 to 1.25 equivalents of curing agent per epoxide equivalent for those curing agents which cure by reacting with the epoxy group of the Sepoxy resin or per hydroxyl group for those curing agents which cure by reacting with the aliphatic hydroxyl groups along the backbone of the epoxy resin.
The advanced epoxy resins of the present invention can be blended with other materials such as solvents or diluents, fillers, pigments, dyes, i WO 89/06662 PCT/US88/04678 flow modifiers, thickeners, reinforcing agents, accelerators and combinations thereof.
These additives are added in functionally equivalent amounts the pigments and/or dyes are added in quantities which will provide the composition with the desired color; however, they arA suitably employed in amounts of from 1 to 200, more suitably from 10 to 100, most suitably from to 100 percent by weight based upon the weight of the resin binder.
Solvents or diluents which can be employed herein include, for example, hydrocarbons, ketones, glycol ethers, chlorinated solvents, esters and combinations thereof. Particularly suitable solvents or diluents include, for example, toluene, benzene, xylene, methyl ethyl ketone, methyl isobutyl ketone, diethylene glycol methyl ether, dipropylene glycol methyl ether, ethylene glycol butyl ether, propylene glycol methyl ether, 1,1,1trichloroethane, DuPont DBE dibasic ester, ethylacetate, propylene glycol t-butyl ether and combinations thereof.
Reinforcing materials which can be employed herein include natural and synthetic fibers in the form of woven, mat, monofilament, multifilament, 0and the like. Suitable reinforcing materials include, glass, ceramics, nylon, rayon, cotton, aramid, graphite and combinations thereof.
Suitable fillers which can be employed IM herein include, for example, inorganic oxides, WO 89/06662 PCT/US88/04678 -16ceramic microspheres, plastic microspheres and combinations thereof.
The advanced epoxy resin compositions of the present invention can be emplbyed in the preparation of coatings, castings, laminates, composites, encapsulants, and potting compositions.
WO 89/06662 PCT/US88/04678 -17- Example 1 Preparation of Glycidyl Ether of Reaction Product of Bisphenol A and Propylene Oxide.
Into a reaction vessel equipped with stirrer, temperture controller, condenser and nitrogen pad containing 500 g of ethylene dichloride was dissolved, at 75 0 C, 172 g (1 OH equiv.) of the reaction product of propylene oxide and bisphenol A in a molar ratio of 2 Sto 1, respectively. Stannic chloride, 5 g (0.02 equiv.) is added and the temperature was raised to reflux, 88 0 C. Epichlorohydrin, 194 g (1.2 equiv.) was added over a 45 minute period from a dropping funnel.
The solution turned black. The reaction mixture was cooled to 700C and 6 ml (0.0166 moles) of a 60 percent aqueous solution of benzyl trimethylammonium chloride and 500 g (2.5 moles) of a 20 percent aqueous solution of sodium hydroxide were added and the reaction mixture cooled to 50°C. Stirring was continued and the mixture maintained at 50°C for 2 hours. The reaction mixture was cooled to 35°C and the aqueous layer was separated from the organic layer. To the organic layer was added an additional 250 g (1.25 moles) of 20 percent aqueous sodium hydroxide and 3 ml (0.008 moles) of a 60 percent aqueous solution of benzyl trimethylammonium chloride catalyst was added. The reaction mixture was heated to and maintained thereat with stirring for 2 hours.
The reaction mixture was cooled to 35°C and the aqueous layer was separated from the organic layer. The organic layer was washed uhree times with 150 ml portions of water. The ethylene dichloride was removed under vacuum in a rotary evaporator at 1500C. The resultant product had an epoxide equivalent weight (EEW) of 301.75, an aliphatic hydroxyl content of 1.86 I I I WO 89/06662 PCT/US88/04678 -18wt. percent and a viscosity of 4040 cps (4.04 Pa.s) at 0
C.
Preparation of Advanced Epoxy Resin.
A diglycidyl ether of bisphenol A having an EEW of 180, 152.7 g (0.85 epoxy equiv.), was blended with 356.2 g (1.18 epoxy equiv.) of the product from A above. This mixture was heated to 80°C at which time 191.2 g (1.68 equiv.) of bisphenol A was added. After the bisphenol A has dissolved, 0.727 g of a 70 wt.
percent methanolic solution of ethyl triphenyl phosphonium acetateeacetic acid complex catalyst was added. The reaction mixture was heated to 150°C and the heat source was turned off. The reaction exotherm caused the temperature to rise to 190°C, which temperature was maintained for 4 hours. The resultant advanced epoxy resin had an EEW of 1991.
Modification of Advanced epoxy resin.
To 50 g (0.025 equiv.) of the advanced epoxy resin prepared in above was mixed 12.5 g of ethylene glycol monobutyl ether in a three neck 250 ml round bottom flask equipped with a temperature controller, condenser, and nitrogen pad. The mixture was heated to 115°C with stirring to dissolve the resin.
A mixture of 11.3 g water, 2.24 g (0.025 equiv.) of dimethylethanol amine and 1.51 g (0.025 equiv.) of 3 0 acetic acid was added to the resin solution at 90 0 C to over a 5 minute period. Heating and stirring was continued for 4.25 hours. The solution was dispersed by the dropwise addition of 56.8 g of water over a minute period resulting in a dispersion containing percent nonvolatiles by weight. The percent nonvolatiles was reduced to 30 percent by the addition WO 89/066-6- PCT/US8/04678 -19of 45 g of water over a period of 10 minutes. The product was nearly transparent with a bluish tinge.
The pH of the product was 6.9, the Ford #4 cup viscosity at 25°C was 15.6 seconds and the volatile organic content (VOC) is approximately 1.6 lbs/gallon (191.7 kg/m 3 Preparation of Coating.
A portion of the modified advanced epoxy resin Sprepared in C above was mixed with a melamine curing agent (CYMEL" M 325 commercially available from American Cyanamide Company) at levels of 15, 20 and 25 phr (parts per hundred parts by weight of the modified advanced epoxy resin). These formulations were coated onto cold rolled steel panels using a drawdown bar.
The coating was cured by baking in an electric convection oven at 400°F (204.4 0 C) for 10 minutes solid epoxy resin).
SOLVENT RESISTANCE was measured by rubbing the coating with a 2-pound (0.9 Kg) ballpein hammer where the hammer head was covered with gauze and soaked in methyl ethyl ketone (MEK). The number of double rubs, pushpull motion, observed uni il a marring of the coating occurs was recorded.
FLEXIBILITY was measured by the wedgebend test according to ASTM D3281-84 and/or the T-bend test J according to ASTM D4145-83.
REVERSE IMPACT was determined by the procedure of ASTM D2794.
The properties are given in Table I.
WO 89/06662 PCT/US88/04678 COMPARATIVE EXPERIMENT A Modification of Advanced Epoxy Resin.
The procedure of Example 1-C was repeated using an aromatic advanced epoxy resin instead of the advanced epoxy resin prepared in Example 1-B. To 200 g (0.103 equiv.) of a diglycidyl ether of bisphenol A advanced with bisphenol A and having an an EEW of 1941 commercially available from The Dow Chemical Company as 667 was added 50 g of ethylene glycol monobutyl ether. The mixture was heated to 125 0 C with stirring to dissolve the resin. A mixture of 46.4 g water (2.58 equiv.), 6.9 g (0.077 equiv) dimethylethanol amine, and 5.9 g (0.098 equiv.) glacial acetic acid was added to the resin solution at 90°C to 95 over a 15 minute period. The mixture was stirred for 4.5 hours at The solution was dispersed by the dropwise addition of 400 g of deionized water over a 1 hour period resulting in a dispersion of the modified advanced epoxy resin.
The product was milky white and opaque. The pH of the product was 6.2, the Ford #4 cup viscosity at 25°C was 14.4 seconds, and the VOC was 1.6 lbs/gal (0.192 kg/1).
2. Preparation of Coating The above dispersion was formulated as described in Example 1-D using 15, 20 and 25 phr of SCYMEL'U 325 as a curing agent. These formulations are coated onto cold rolle steel panels using a drawdown bar. The coating was cured by baking in an electric convection oven at 400 0 F (204.4 0 C) for 10 minutes. The properties of the coatings prepared from this modified advanced epoxy resin are given in the Table.
i I :i WO 89/06662 PCT/US88/04678 COMPARATIVE EXPERIMENT B The procedure of Example 1-A was repeated using an advanced epoxy resin derived from a blend of aliphatic liquid epoxy resin and aromatic liquid epoxy resin.
Preparation of Advanced Epoxy Resin A diglycidyl ether of bisphenol A having an EEW 1 of 180, 300 g (1.67 equiv.) was blended with a diglycidyl ether of polypropylene glycol having an EEW of 320, 200 g (0.625 equiv.) and the blend was reacted with bisphenol A, 151 g (1.32 equiv.). The reactants were blended and heated to 80°C. After the bisphenol A was dissolved, 0.95 g of a 70 wt. percent methanolic solution of ethyl triphenyl phosphonium acetateeacetic acid complex catalyst was added. The reaction mixture was heated to 150°C and the heat source turned off. The reaction exotherm caused the temperature to rise to 185°C, which temperature was maintained for 4 hours.
The resultant advanced epoxy resin had an EEW of 1886.
Modification of Advanced Epoxy Resin The advanced epoxy resin prepared above was modified as described in Example 1-C. To 200 g (0.106 equiv.) of the advanced epoxy resin prepared in comparative experiment B-1 above was added 50 g of ethylene glycol monobutyl ether. The mixture was heated to 125*C with stirring to dissolve the resin. A mixture of 47.7 g (2.65 equiv.) water, 7.9 (0.079 quiv.) dimethylethanol amine, and 6 g (0.1 equiv.) glacial acetic acid was added to the resin solution at 90 0 C to 95 0 C over a 15 minute period. The mixture was stirred for 4.5 hours at 900C. The solution was WO 89/06662 PCT/US88/04678 -22dispersed by the dropwise addition of 400 g deionized water over a 1 hour period resulting in a dispersion of the advanced epoxy resin. The product was creamy white and opaque. The pH of the product was 6.8, the Ford #4 cup viscosity at 25°C was 14.1 seconds, and the VOC was 1.6 lbs/gal. (0.192 kg/1). The resultant dispersion settled out after one week, but it was readily redispersible.
Preparation of Coating The dispersion prepared in comparative experiment B-2 above was formulated as described in Example 1-D using 15, 20 and 25 phr of CYMEL" T 325 as a curing agent. These formulations were coated onto cold rolled steel panels using a drawdown bar. The coating was cured by baking in an electric convection oven at 400°F (204.4°C) for 10 minutes. The properties of the coatings prepared from this modified advanced epoxy resin are given in the Table.
WO 89/06662 WO 8906662PCT/US88/04678 23- Amount Rev. Impact Ex. or OIL Flexi- MEK Comp. Curing bility Double phr in-lbs kg-cm 1 15 T3 80 92 1 20 T3 72 83 1 25 T3 72 83 T3 70 81 T460 69 4o T5 40 46 B*15 T14 80 92 12 2020 T14 60 69 B* 25 T5 50 58 18 -Nr'ot an examplJe Q; the present ivenition.
aThe lower the T -value, the more flexible coating.
the

Claims (9)

1. A modified advanced epoxy resin, which results from reacting an advanced epoxy ,.sin which r~esults from r'ea~tirng an epoxy resin composition comprising at least one epoxy vesin having an average of more than one, but not more than two vicinal epoxy groups per molecule and which contains- at least one oxyalkylene or substitute M6eV e, oxyalkylene group per7 molecule; at least one compoun4 having two aromatic hydroxyl groups per Mol~olde; wherein components and are employed in amou~nts wh3.oh providte a ratio of aromatic hydroxyl groups per epoxy group of from 0.005:1 to 200:1; with a nitroger'-oQrtaining compound selected fr'om primary inonoatnines; secondary moooainines; tertiary rnonoardines; (4)hyrOy2 8us1it ~seconaj or-. tertiary monoamlnes; or any cobnti (8l-1)t V 1 -24 a- hydroxyl substituted primary, tertiary monoamines; ammonia; or any combination of cc~nponents or secondary *9 0O 0e 0* S S@ SS SO S S S 5 .55. S S *05S SO 59 S U S S S 955505 9 *SSS 5 5* U ge 5 9 S S US 5 Ri~ I.- 1. i I i WO 89/06662 PCTIUS8810467867 wherein components and are present in an amount such that the ratio of amine groups contained in component to epoxy groups contained in component is from 0.1:1 to 1.1:1.
2. A modified advanced epoxy resin of Claim 1 wherein component further comprises at least one epoxy resin which has an average of more than one but not more than two vicinal epoxy groups per molecule and which is different from the epoxy resin of wherein components A-l-a) and are present in amounts such that from5 equivalent percent of the epoxide groups are derived from component and from 5 to 95 equivalent percent of the epoxide groups are derived from component A- Q iC cl
3. A- advanced epoxy resin of Claim 2 wherein component is an epoxy resin or mixture of epoxy resins represented by the following formula I Formula I 0 0 H 2 C C-CH2- CH2 C CH 2 R I R R wherein each R is independently hydrogen or an alkyl group having from 1 to 4 carbon atoms; Z is a divalent aromatic group represented by the following formulas II and III I I i i WO 89/06662 PCT/US88/04678 -26- Formula II Formula III (X) 4 (X)4 (X)4 wherein A is a divalent hydrocarbyl group having from 1 to 12 carbon atoms, -S02-, or each X is independently hydrogen, a hydrocarbyl or hydrocarbyloxy group having from 1 to 12 carbon atoms, or a halogen; n is zero or 1; each Z' is independently a group represented by the following formula IV Formula IV -CH-CH- 20I I R 2 R1 wherein each R1 and R2 are independently hydrogen or a hydrocarbyl or hydrocarbyloxy group having 1 to 12 carbon atoms or a -CH2-0-R 3 group wherein R3 is a hydrocarbyl group having from 1 to 12 aarbon atoms; and each m and m' independently has a value from 1 to component is an epoxy resin or mixture of epoxy resins represented by the following formulas VII, VIII or IX or combinations thereof; 00 Formula VII 0 H 2 C -C-OH 2 R 0 (X) 4 OH 0 CH2-C-CH 2 R (X) 4 0 0 0 CH 2 -C CH 2 ni R Formula V III MX 4 H 2 C- C-CH2-O (X) 4 (X) 4 0 0 CH 2 -C OH 2 I it WO 89/06662 PCT/US88/04678 -28- Formula IX o o H2C C CH 2 0 (-CHCH-0) m CH2 -C -CH 2 I I i I R R2 R1 R wherein A, R, RI, R 2 X, m and n are as defined above and n' has an average value from zero to component is a compound or a mixture of compounds represented by the following formulas V and VI Formula V (X) 4 K- OH Formula VI (x) 4 (X) 4 wherein A, X and n are as defined above; and component is a volatile monoamine. i WO 89/06662 PCT/US88/04678 -29- A moO Oie d
4. An advanced epoxy resin of Claim 3 wherein component is a diglycidyl ether of the reaction product of bisphenol A with ethylene oxide, propylene oxide, butyletse oxide, phenyl glycidyl ether, butyl glycidyl ether or a combination thereof; component is a diglycidyl ether of bisphenol A, bisphenol F or a combination thereof; and component is bisphenol A, bisphenol F or a combination thereof. A modified advanced epo 'y resin of Claim 1 or 2 which has additionally been reacted with a monocarboxylic acid.
6. A curable composition which comprises, a advanced epoxy resin of Claim 1 or 2 and a .curng quantity of a suitable uring agent for saidadvanced quantity of a suitable curing agent for said~advanced epoxy resin. a (o diC' d
7. A curable composition which comprisesqan advanced epoxy resin of Claim 5 and auring quantity Sof a suitable curing agent for said advanced epoxy 2 resin.
8. A cured product resulting from curing the curable composition of Claim r I i. 1 iii:i i
9. A modified advanced epoxy resin substantially as hereinbefore described with reference to Example 1. A curable composition substantially as hereinbefore described with reference to Example 1. DATED: 4 March, 1991 THE DOW CHEMICAL COMPANY By their Patent Attorneys: PHILLIPS ORMONDE FITZPATRICK nuk 4,4~c 6 6* 6O 6 6 S 6 0 S 6* 6 6 6f -y ;-L~LYI-~t-i I INTERNATIONAL SEARCH REPORT International Application No, PCT/US 8 8/0 4 678 I. CLASSIFICATION OF SUBJECT MATTER (if several classification symbols apply, indicate all) 6 According to Internaonal Patent Classification (IPC) or to both National Classification and IPC IPC 4 C08G 59/02, 16 t q. pi. /t;4c/R1 AR a i n i' "3 i a1 R/ 03, 111, 121 II. FIELDS SEARCHED J ill 1 Minimum Documentation Searched 7 Classification System Classification Symbols U.S. CL. 525/481, 488, 504, 510, 523, 531; 528/103, 104, 111, 121 Documentatlon Searched other than Minimum Documentation to the Extent that such Documents are Included In the Fields Searched B III. DOCUMENTS CONSIDERED TO BE RELEVANT 9 Category Citation ao Document, tl with indication, where appropriate, of the relevant passages 12 Relevant to Claim No. 1i A US, A, 3,379,791 (LARSON) 23 APRIL 1968; ALL SEE ENTIRE DOCUMENT. A US, A, 3,937,679 (BOSSO) 10 FEBRUARY 1976; ALL SEE ENTIRE DOCUMENT. A US, A, 3,962,165 (BOSSO) 08 JUNE 1976; ALL SEE ENTIRE DOCUMENT. X US, A, 3,984,299 (JERABEK) 05 OCTOBER 1976; ALL SEE ENTIRE DOCUMENT. A US, A, 4,176, 221 (SHIMP) 21 NOVEMBER 1979 ALL SEE ENTIRE DOCMENT. A US, A, 4,339,369 (HICKS) 13 JULY 1982; ALL SEE ENTIRE DOCUMENT. A US, A, 4,507,461 (BOWDITCH) 26 MARCH 1985; ALL SEE ENTIRE DOCUMENT. A US, A, 4,596,861 (SHEIH) 24 JUNE 1986 ALL SEE ENTIRE DOCUMENT. Special categories of cited documents; 1o later document publishd alter the international filing dale document defining the general state of the art h;'ch is not or priority date and not In conflit with the application but considered to be of particular relevance €vtedr to understand the plriple of. thnory underlying the "E earlier document but publishad on or alter the international document f particular relevance; the claimed invention filing date Cannot be considered novel or cannot be considered to document which may throw doubts on ~iorilt claim(s) or involve an inventive step which Is cited to establish the publicatonl date of another document of particula relevance; the claimed invention cilatlort or other special reason (as specified) cannot be considered to involve an inventive step when the document referring to an oral disclosure, use, exhibition or document is combined with one or more other such docu. other means ments, such corrbination being obvious to a person skilled document published prior to the internatiorial filing date in the art later than the priority date claimed document member o the same patent family IVI CERTIFICATION Date of the Actual Completion of the International Search Date o Mailing of this International Search Report 09 MARCH 1989 0 4MAY 198 International Searching Authority $Igna!re of Authort aOfcet IoCTSA/US A. NIELSENsv, Form PCT/lSA 10t (Ond $hml) (Rev,. t.7) I 0 4 International Application No. PCT/US 88 /04678
111. DOCUMENTS CONSIDERED TO BE RELEVANT (CONTINUED FROM THE SECOND SHEET) Category Citation ol Document, with Indication, where appropriate, ol the relevant Passages Relevant to Claim No A US, A, 4,608f405 (DEGOOYER) 26 AUGUST 1986. SEE ENTIRE DOCUMENT. GB, A, 2,137,205 (DOW) 03 OCTOBER 1984; SEE ENTIRE DOCUMENT. ALL ALL Form ICT/14IN21 (40la shoo) (Revt 1t47)
AU30382/89A 1988-01-13 1988-12-28 Modified advanced epoxy resins Ceased AU612794B2 (en)