AU597063B2 - Process for preparation of resin and resin obtained - Google Patents

Process for preparation of resin and resin obtained Download PDF

Info

Publication number
AU597063B2
AU597063B2 AU73372/87A AU7337287A AU597063B2 AU 597063 B2 AU597063 B2 AU 597063B2 AU 73372/87 A AU73372/87 A AU 73372/87A AU 7337287 A AU7337287 A AU 7337287A AU 597063 B2 AU597063 B2 AU 597063B2
Authority
AU
Australia
Prior art keywords
resin
formaldehyde
carbohydrate
reactor
reaction
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Ceased
Application number
AU73372/87A
Other versions
AU7337287A (en
Inventor
Tito Viswanathan
Donald H. Westermann
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
CHEMICAL PROCESS Corp
Original Assignee
CHEMICAL PROCESS CORP
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Priority claimed from US06/839,513 external-priority patent/US4692478A/en
Application filed by CHEMICAL PROCESS CORP filed Critical CHEMICAL PROCESS CORP
Publication of AU7337287A publication Critical patent/AU7337287A/en
Application granted granted Critical
Publication of AU597063B2 publication Critical patent/AU597063B2/en
Anticipated expiration legal-status Critical
Ceased legal-status Critical Current

Description

2/87 17063 4947-Pl/GD/AP/1003T/.
ASRL597063 1 ;i ci i- PATENTS ACT 1952 COMPLETE SPECIFICATION
(ORIGINAL)
FOR OFFICE USE Application Number: Lodged:
I
Complete Specification Lodged: Accepted: Published: Priority: Related Art: 1,
.I"
TO BE COMPLETED BY APPLICANT Name of Applicant: Address of Applicant: Actual Inventor: Address for Service: CHEMICAL PROCESS CORPORATION 5300 Sutton Place So.
Greenfield, Wisconsin, 53221, United States of America TITO VISWANATHAN DONALD WESTERMANN ARTHUR S. CAVE CO.
Patent Trade Mark Attorneys Goldfields House 1 Alfred Street SYDNEY N.S.W. 2000
AUSTRALIA
vated the pH of s~-~uI Complete Specification for the invention entitled PROCESS FOR PREARATION OF RESIN AND RESIN OBTAINED.
The following statement is a full description of this invention including the best method of performing it known to me:- _rh _i 3 -1- ASC 49 B 2 PROCESS FOR PREPARATION OF RESIN AND RESIN OBTAINED Technical Field The present invention relates to a process for the production of a thermosetting resin for use in binding solid lignocellulosic materials to form products, such as particle board, and to the novel resin obtained.
Background Art Urea-formaldehyde and phelol-formaldehyde condensation resins are the major types of thermosetting resins currently used as adhesives for binding together solid lignocelluiosic materials, including wood, to form useful products. The resins generally are provided as aqueous products containing high solid levels or as powders which may be dissolved in water or applied directly to the lignocellulosic particles prior to hot pressing to form particle board. Even though most of the formaldehyde employed in forming the resin reacts with the urea or the phenol and forms part of the polymeric adhesive resin, some free formaldehyde remains which can volatilize from the final product into the immediate environment, Liberation of formaldehyde from the nd product may also result from the hydrolysis of the resin. Formaldehyde has been implicated as a carcinogen and its presence -in the environment poses a potential public health problem.
I p- 3 Therefore, it is desirable to have adhesives that do not either contain formaldehyde as an ingredient or which will release formaldehyde upon hydrolysis.
The basic raw materials used in most commercially available condensation resins are derived from petroleum and natural gas. Since the prices of these non-renewable resource materials have increased, attempts have been made to replace them with less expensive materials. For example, carbohydrates, such as sugars and starches, have been employed as ingredients in binders for solid lignocellulosic materials to produce water proof plywood and particle boards.
In the Viswanathan et al. U.S. Patent 4,524,164, a method is disclosed for binding solid lignocellulosic materials using an adhesive which is made from readily available carbohydrates and which does not contain formaldehyde. In the patent, the reactants including a carbohydrate source, preferably whey, an inorganic acid and a catalyst, are all added simultaneously to a batch reactor. The simultaneous addition of all the reactants precludes any advantage to be gained in resin quality i and/or economy of production which might be derived by Iseparating the desirable from the undesirable reactions through successive additions of reactants or by proper choice of optimum process parameters, temperature, pressure and concentrations.
The Viswanathan process and resin are valuable improvements in the field of making particle board, but it 1 would be even more desirable to have a process in which the carbohydrate, which is used as the raw material, does not degrade to undesirable products and in which the resin obtained will cross-link without requiring the addition of polyfunctional cross-linking agents.
It is the primary object of this invention to disclose a superior process for the preparation from nonpetroleum raw materials of a non-formaldehyde containing thermosetting resin which is both useful in the binding of materials and as a molding compound.
-4- 4 It is a further object to disclose a novel, water soluble, storage stable, formaldehyde-free thermosetting resin for use in binding lignocellulosic materials to prepare products, such as particle board.
The process of the present invention basically comprises two steps or phases.
In the first step, an aqueous solution of a carbohydrate containing material, preferably whey or whey permeate, is reacted with a mineral acid, such as sulfuric acid, hydrochloric acid or phosphoric acid, under very low pH conditions at a temperature from about 100 0 C to about 225 0 C, to rapidly hydrolyze the polymers, oligimers or disaccharides in the carbohydrate containing material to simple sugars which are then converted to polymerizable reactants such as HMF and dimers and oligimers of HMF and related compounds.
In the second step, the reactive compounds, including the polymerizable monomers, are reacted with ammonia under less acidic conditions to cause them to react, polymerize and partially cross link to form a water soluble, storage stable, thermosetting resin which upon added heating will further cross link and set to an insoluble solid. Preferments follow.
The exact mechanisms by which the thermosetting resins are formed are not known, however, it is known that carbohydrates are sensitive to extremely acidic or alkaline conditions. For example, the principal carbohydrate of whey, lactose, readily degrades when exposed to temperatures in excess of 100 0 C into not only its hydrolysis products, glucose and galactose, but also hydroxymethylfurfural and other degradation products. In addition to the desirable hydroxymethylfurfural (HMF), Strecker degradation and other charred products are produced.
It is an object of the first step of the process of the present invention to control the degradation so that the undesirable degradation products are either not form- A ed or only formed in small amounts. In the second step the desirable degradation products, the polymerizable monomers, are polymerized under less acidic conditions.
From the description which follows, it will be apparent to those skilled in the art that the process and resin of the present invention possess numerous advantages over prior known I processe. anU resins.
In the preferred embodiment of ,ne invention, whey or whey permeate is the preferred carbohydrate source, however, a' practically any source of starch, dextrins and sugars may be ta used. The use of whey or whey permeate is preferred because, in addition, to providing an economical source of carbohydrates the use of whey or whey permeate alleviates a long standing environmental problem by using an abundant waste material t:o prepare a useful product. The use of whey or whey permeate is further preferred because it contains protein and other nitrogen containing products that appear to cooperate in providing a resin which is superior to those obtained from a pure carbohydrate source such as lactose.
In the preferred practice of the process, in the first step an aqueous preparation of whey permeate, containing from about 30% to about 95% solids in water, is heated in a reactor ,r i to about 140 to about 250°C in about 10 to about 20 minutes in the presence of sufficient mineral acid, preferably sulfuric acid, to produce a pH of about 0.5 to about 2.0. Under these conditions the lactose in the whey is hydrolyzed to glucose and galactose which in turn are degraded to HMF and other "b pjk 0246g/MS 1 1 -7 1 5a polymerizable reactants. In the second step, at about 145 0
C,
sufficient ammonia gas is introduced into the closed reactor to produce a final pH of 2.0 to 5.0, preferably 3.0 to whereupon the polymerizable reactants are polymerized to the desired resin.
It is believed that the following major reactions take place in the formation of the resin:
SI
t t 0246g/MS 1 I i -3ura~-- -arx9 Acid Lactose -0 Heat Galactose Glucose Acid Heat Water Polymerizable reactants Water
NH
3 Resin 9 t 4 4 4 t 4 t o 4 4t 4 a 1 4) l j The preferred mineral acid is sulfuric acid, however, other mineral acids, including hydrochloric acid or phosphoric acid can also be used. The only mineral acid not recommended is nitric acid which is known to oxidize the aldehyde groups of sugar monomers to carboxylic acid groups.
Although liquid ammonia can be used, the use of gaseous ammonia is preferred to minimize the dilution of the reactants.
The dry whey permeate will usually contain about 20 80-90% lactose and small amounts of protein and other nitrogen containing compounds. It is commercially available from many sources.
The two step process can be operated in a continuous mode by using a compartmented reactor which simulates "plug flow" reactor conditions. In a compartmented reactor, the time for completing the major reactions which comprise the complete process can be, as little as, five to ten minutes.
Exoerimental Procedures In the examples which follow, the technique described to follow the progress of the reactions and to deduce the perceived mechanism of the successive reactions which occur, is based on the solubility of the reactants and products in a limited quantity of methanol. For all measurements of the methanol insoluble products (hereafter called one gram of the 7 reactant or product solids was dispersed in one hundred milliliters of methanol. The solid was dispersed in the methanol and the suspension filtered. The insoluble residue was recovered, dried and weighed and duly recorded as M.I.P. or the percentage of the original gram of solids. M.I.P. was plotted as a function over the course of the reaction.
Upon initial suspension of the whey solids in methanol the degree of M.I.P. was approximately 90%. This is consistent with the solubility of lactose in methanol under these conditions of limiting solvent volume as noted by a measurement of pure lactose solubility under these conditions, Upon addition of the sulfuric acid to establish a pH of 0.5 followed by heat up of the reactor a sample taken about one minute later produced an M.I.P.
of 50 to 53%, This value of M.I.P. is consistent with the solubility of glucose and galactose in methanol as confirmed by measurements of the solubilities of pure compou.ds under this restricted solvent condition. These measurements, along with Infra Red Spectrophotometry, confirm the presence of the monosaccharides in the reaction mix after the first several minutes of batch reactor S' heatup.
In the next few minutes of the first step, the monosaccharides are dehydrated to hydroxymethylfurfural (HMF), dimers and oligimers of HMF and other dehydration products. At this stage, the M.I.P. drops to a level of about 20%. Tt is known that HMF is completely soluble in methanol. Therefore, a value of 20% insoluble solids indicated that most of the monosaccharides had been converted to highly methanol- soluble HMF and/or dimers of HMF, which was confirmed by tIR. (Infra Red) and N.M.R.
(nuclear ma netic resonance) spectroscopy.
When the minimum amount of M.I.P. is produced the second step of the process is initiated by injecting ammonia gas into the stirred heated reactor or the appropriate compartment of a compartmented reactor, A very U. i i I 8 rapid polymerization takes place as evidenced by the rapid rise in the M.I.P. to a level of about 70% to about A measurement of the molecular weight of the polymer produced at this time shows that molecular weights in excess of about 5,000 are not soluble in methanol under the solvent restricted test conditions. Sufficient ammonia is preferably added to raise the pH to a level of because evaluation of finished products shows that finished resin with a pH of about 4.0 possesses the optimum characteristic for particle board manufacture including high strength, water solubility of the uncured resin S° and water resistance of the cured resin.
o v The final phase, involving complete polymerization 0 0 g and cross linking of the resin, occurs as the result of 0. 15 heating in the preparation of the final product, e.g.
Sparticle board. By experimentally controlling the time o. dwell in the reactor, the degree of polymerization in the reactor, in contrast to the degree of cross linking in the press, can be controlled. In the batch reactor at 4 0 20 145 C about 5 minutes is required for the final cross- Slinking. Consistent with the previous M.I.P. measurements the value of M.I.P. continued to increase as the polymerization and cross linking progressed. Indeed it is possible to cause the resin to solidify in the reactor 25 if held 10 or more minutes under the described conditions.
To determine the conditions required for a proper continuous reactor production of the resin in two steps, comprising the previously described reactions, the batch data were analyzed to obtain kinetic constants. These constants then allowed establishing the desired continuous reaction parameters for resin production.
Analysis of the batch experimental data showed the following equation adequately described the first hydrolysis reaction: Lactose Galactose Glucose 9 The reaction was found to be first order with respect to both concentration of lactose and hydrogen ion concentration. An energy of activation of 85 KiloCalories per gram mole indicates a relatively high sensitivity to temperature. At 100 0 °C the reaction rate would double for a 3 0 C rise in reaction temperature. Therefore, it is obvious that the initial hydrolysis of lactose can be accomplished very rapidly.
Calculations based on data gathered from batch reactior. shows the energy of activation of the monosaccharide dehydration, the second reaction in the process, to be very low, about 10 kcal. gm. mole. The reaction is first order with respect to concentration at a pH of 0.5 and first order with respect to hydrogen ion concentration at the pH range around 0.5 to 1.0. The fact that the anticipated dehydration occurs in this second reaction is confirmed by calculations that show the availability of 76% of the three molecules of water from the cyclization reaction to HMF when allowing for one molecule of water per mole to be added to lactose upon hydrolysis to glucose and galactose. The calculation is based on the decrease in solids content or conversely the increased water content which occurs during the course of the entire reaction.
The third reaction in the process, the polymerization of the dehydrated monomers, HMF and its derivatives, with gaseous ammonia is very rapid, less than one minute at 145 0 C. The M.I.P. increases by 50 to 70%. The II ammonia reacts with the reactive intermediates and raises the pH. The rate of reaction is so fast that successive samples could not be taken from a batch reactor for subsequent evaluation.
After the M.I.P. has risen very rapidly due to the introduction of the gaseous ammonia the insolubility in methanol, continues to rise as the result of the crosslinking taking place. If heating is continued within approximately the next ten minutes after the M.I.P. has increased to 50 to 70% the M.I.P. increases to 80-85% and, the resin solidifies completely. Therefore, the continued polymerization and cross linking required in making particle board in the board press can be controlled by the time the resin is held in the reactor during this last stage.
The practice of the invention is further illustrated by the following examples.
Example 1 233 gram of dried whey permeate was added to a 500 ml high pressure Parr heated reactor containing 90.0 grams of fresh water to form a suspension of 72% solids. Next 9.7 ml. of 95% sulfuric acid was added.
The pH of the reaction mix was 0.5. The reactor was sealed and the contents were vigorously stirred with a flat bladed turbine agitator. It took about 15 minutes for the contents to rise to the control temperature of 145°C. After 20 minutes, 3.04 gram of gaseous ammonia was introduced into the reactor under pressure. The pH was then about 4.0. The contents of the reactor were held at 145 0 C for an additional 10 minutes. The profiles of t.he M.I.P. of the reactor contents and the pH of the contents were measured by withdrawing small aliquots during the course of reaction. Performance of the resin in finished particle board is shown in Table 1.
j Resin Press Temperature co TABLE 1.
Density Of Internal Bond Board Lb/Ft Strength,p.s.i.
Press Time Swelling in water(25 hr.,) Dry Strength p.s.i.
Example Exampl e Example 7% Example 7% Example 7%" Example 7% 180 180 180, 180 180 18 0 5 min..
5min.
6 min.
6 min.
6 min.
6 min.
89 109 102 106 20.0 20.0 12 Example 2 233 gram of "Staleydex 95" (trademark of A.E. Staley Co., Decatur, Ill.) a commercial dextrin was introduced into a 500 ml Parr reactor containing 90.3 ml. of water and 9.7 ml. of 95% sulfuric acid. The pH of the contents of the reaction mix was 0.5. The reactor was sealed and the contents were stirred as described in example 1 while simultaneously heating to 145 0 C. The generation of M.I.P. was measured as described. 3.04 grams of gaseous ammonia was introduced at 17 minutes reaction time to increase the pH of the contents to 4.0. The reaction was Scontinued for an additional 5 minutes. Particle board 9 0 made with the resin is described in Table 1.
0 000 Example 3 233 gram of pure food corn starch was introduced into a 500 ml Parr reactor containing 9.7 ml of 95% sulfuric acid and 90.3 ml of water. The oH of the reaction mix was 0,5. The reactor was sealed and the contents heated to 145 0 C while simultaneously stirring. After 17 4 20 minutes 3.04 grams of gaseous ammonia was introduced o"0" 0 under pressure to bring the pH up to 4.0. The contents were then heated an additional 5 minutes. The generation oo, of M.I.P. was measured as described. Properties of particle board made from the resin are shown ir Table 1.
K.imple 4 116,5 grams of "Staleydex 95" and 116.5 grams of whey permeate were introduced into a 500 ml rtgtor whih contained 9.7 ml of sulfuric acid and 90.3 mi of weter, The pH of the reaction mix was 0.5. The reactor was sealed and heated to 145°C while simultaneously stirring. After 17 minutes 3.04 grams of gaseous ammonia was Introduced to bring the pH up to 4.0, The reaction mix~ cure was heated fcr an additional 5 minutes Properties of particle board made with resin are shown in Table o1 Example Carbohydrate consisting 1.16.5 grams of -tarch and 116.5 gqam o£ whey permeate were te 13 sulfuric acid, water, whey and ammonia as described in Example 4. The properties of particle board made with the resin are shown in Table 1.
Example 6 Resin was produced as cited in example 1 except the time the contenits were held in the reactor at the end of the reaction was varied from 0 to 8 minutes. It was found that holding the resin in the reactor up to minutes inc.reased the desirable properties of particle board made with the resin but that holding the resin longer had a detrimental effect on the finished products, Example 7 233 grams of whey permeate was added to a 500 ml high pressure Parr reactor containing 90 grams of fresh water. The pH of the contents was adjusted to 0.5 by the addition of~ concentrated hydrochloric acid. The reactor was sealed a.nd while the contents was stirred, it was Vheated to 145 0 C. When the methanol insoluble reactants of the mix reached a miua.murn of 22%, 21 minutes after starting the reaction, gaseous ammonia was added to raise the pH to 4.0. The results obtained were comparable to those- obtained with the resin of Example 1.
Example 8 The process off Example 7 was repeated except that phosphoric acid was used instead of hydrochloric acid.
The results were comparable to those obtained with the resin of Example I.
It will be readily apparent to those skilled in the art that the foregoing descripti.on has been for purposes of illustration only and that a number of changes and modifications may be made withNat departing from the spilt and scope of the present invention. Therefore, it is intended that the inventlon not be limited except by the claims which follow:

Claims (9)

1. The process for preparing a formaldehyde-free thermosetting resin, which process comprises reacting an aqueous preparation containing a carbohydrate at an elevated temperature with sufficient mineral acid, to produce a pH of to 2.0, and convert the carbohydrate to polymrerizable reactants, and then reacting at an elevated temperature the thus obtained reactants with ammonia to produce a final pH of to 5.0 to form a storage stable, water soluble, thermosetting resin which can be further cross-linked by exposure to heat. S
2. The process in claim 1 in which the carbohydrate is whey permeate.
3. The process of claim 1 in which t!L& :ous preparation contains 30 to 95 percent solids by weight of carbohydrate.
4. The process of claim 1 in which the mineral acid employed is sulfuric acid.
The process of claim 1 in which sufficient mineral acid is employed to adjust the pH to about
6. The process of claim 1 in which sufficient ammonia is employed to adjust the pH of the reaction mixture to 3.0 to
7. A formaldehyde-free resin prepared by the process of claim 1.
8. A product containing lignocellulosic materials bound together with a formaldehyde-free resin prepared by the process of claim 1. I^,.0246g/MS b l^ r ~y- I- 15
9. A process for preparing a formaldehyde-free thermosetting resin, substantially as herein described, with reference to any one of Examples 1 to 8. DATED this 26th day of February, 1990. CHEMICAL PROCESS CORPORATION By Its Patent Attorneys ARTHUR S. CAVE CO. 0246g/MS j
AU73372/87A 1986-03-14 1987-05-22 Process for preparation of resin and resin obtained Ceased AU597063B2 (en)