AU2006285062B2 - Modified landplaster as a wallboard filler - Google Patents

Modified landplaster as a wallboard filler Download PDF

Info

Publication number
AU2006285062B2
AU2006285062B2 AU2006285062A AU2006285062A AU2006285062B2 AU 2006285062 B2 AU2006285062 B2 AU 2006285062B2 AU 2006285062 A AU2006285062 A AU 2006285062A AU 2006285062 A AU2006285062 A AU 2006285062A AU 2006285062 B2 AU2006285062 B2 AU 2006285062B2
Authority
AU
Australia
Prior art keywords
calcium sulfate
slurry
coating
dispersant
gypsum
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Ceased
Application number
AU2006285062A
Other versions
AU2006285062A1 (en
Inventor
David R. Blackburn
Qingxia Liu
Michael P. Shake
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
United States Gypsum Co
Original Assignee
United States Gypsum Co
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Priority claimed from US11/217,039 external-priority patent/US20070044687A1/en
Application filed by United States Gypsum Co filed Critical United States Gypsum Co
Publication of AU2006285062A1 publication Critical patent/AU2006285062A1/en
Application granted granted Critical
Publication of AU2006285062B2 publication Critical patent/AU2006285062B2/en
Ceased legal-status Critical Current
Anticipated expiration legal-status Critical

Description

WO 2007/027530 PCT/US2006/033297 MODIFIED LANDPLASTER AS A WALLBOARD FILLER CROSS REFERENCES TO RELATED APPLICATIONS This application is a continuation-in-part of U.S. Serial No. 11/217,039 filed August 31, 2005, entitled "Modified Landplaster as a Wallboard Filler," herein incorporated by reference. This application is related to co-pending U.S. Serial No. 5 11/152,317, entitled "Modifiers for Gypsum Slurries and Method of Using Them", U.S. Serial No. 11/152,418 entitled "Gypsum Products Utilizing a Two-Repeating Unit System and Process for Making Them", and U.S. Serial No. 11/152,661, entitled "Fast Drying Gypsum Products", all filed June 14, 2005, and herein incorporated by 10 reference. This application is further related to co-pending U.S. Serial No. 11/450,068, entitled "Modifiers for Gypsum Slurries and Method of Using Them", and U.S. Serial No. 11/449,924, entitled 15 "Gypsum Products Utilizing a Two-Repeating Unit System and Process for Making Them", both filed June 9, 2006 and herein incorporated by reference.
WO 2007/027530 PCT/US2006/033297 FIELD OF THE INVENTION The present invention is directed to a composition utilizing a coated landplaster as a filler in gypsum slurries. More specifically, landplaster is coated with a coating that is less soluble 5 than stucco to reduce or delay its ability to catalyze crystallization reactions. BACKGROUND OF THE INVENTION Gypsum-based building products are commonly used in construction. Wallboard made of gypsum is fire retardant and can be 10 used in the construction of walls of almost any shape. It is used primarily as an interior wall and ceiling product. Gypsum has sound deadening properties. It is relatively easily patched or replaced if it becomes damaged. There are a variety of decorative finishes that can be applied to the wallboard, including paint and wallpaper. Even with 15 all of these advantages, it is still a relatively inexpensive building material. Gypsum is also known as calcium sulfate dihydrate, terra alba or landplaster. Plaster of Paris is also known as calcined gypsum, stucco, calcium sulfate semihydrate, calcium sulfate half 20 hydrate or calcium sulfate hemihydrate. Synthetic gypsum, for example, that which is a byproduct of flue gas desulfurization processes from power plants, may also be used. When it is mined, raw gypsum is generally found in the dihydrate form. In this form, there are two water molecules associated with each molecule of 25 calcium sulfate. To produce the hemihydrate form, the gypsum is 2 WO 2007/027530 PCT/US2006/033297 calcined to drive off some of the water of hydration by the following equation: CaSO 4 .2H 2 0->CaSO 4 .1/2H 2 0 + 3/2H 2 0 A number of useful gypsum products can be made by 5 mixing the stucco with water and permitting it to set by allowing the calcium sulfate hemihydrate to react with water to convert the hemihydrate into a matrix of interlocking calcium sulfate dihydrate crystals. As the matrix forms, the product slurry becomes firm and holds a desired shape. Excess water must then be removed from the 10 product by drying. Significant amounts of energy are expended in the process of making gypsum articles. Landplaster is calcined to make stucco by heating it to drive off water of hydration. Later the water is replaced as the gypsum sets by hydration of the hemihydrate to the 15 dihydrate form. Excess water used to fluidize the slurry is then driven from the set article by drying it in an oven or a kiln. Thus, reducing the amount of water needed to fluidize the slurry turns into a monetary savings when fuel requirements are decreased. Additional fuel savings would result if the amount of material that required calcining 20 were reduced. Attempts have been made to reduce the amount of water used to make a fluid slurry using dispersants. Polycarboxylate superplasticizers are very effective in allowing water reduction and where water reduction results in increased density, a strength increase 25 -is achieved. These materials are relatively expensive. When used in large doses, polycarboxylate dispersants can be one of the single, most expensive additives in making gypsum products. The high price of this component can overcome the narrow margins afforded these products in a highly competitive marketplace. 3 WO 2007/027530 PCT/US2006/033297 Another disadvantage associated with polycarboxylate dispersants is the retardation of the setting reaction. Gypsum board is made on high speed production lines where the slurry is mixed, poured, shaped and dried in a matter of minutes. The board must be 5 able to hold its shape to be moved from one conveyor line to another to put the board into the kiln. Damage can occur if the boards have not attained a minimum green strength by the time they are cut to length and handled during the manufacturing process. If the board line has to be slowed down because the board is not sufficiently set to 10 move on to the next step in the process, production costs are driven up, resulting in an economically uncompetitive product. Modifiers have been found that increase the efficacy of the dispersant in fluidizing the slurry, allowing the modifier to replace a portion of the expensive dispersant while still reducing water demand. 15 However, it has been found that the modifier does not work consistently, depending on how and when it is added to the slurry. Thus, there is a need for a delivery vehicle to carry the modifier to the slurry in a manner that allows it to perform consistently so that the amount of dispersant can be reduced. 20 The use of fillers that are easily fluidizable in water have been considered as another method of reducing fuel demand. However, one of the important properties of gypsum products, and especially gypsum panels or wallboard, is its fire resistance. Calcium sulfate dihydrate is approximately 20% water by weight. Replacing a 25 portion of the calcined gypsum with fillers-that are less fire retardant diminishes this property in the finished product. Many fillers also reduce the compressive strength and the nail pull strength of wallboard. 4 WO 2007/027530 PCT/US2006/033297 Landplaster has been used as a filler in gypsum products. It is also fire retardant, inexpensive, readily available and reduces the amount of calcined gypsum that is needed, but it also has disadvantages. Calcium sulfate dihydrate used in sufficient quantities 5 to act as a filler also acts.as a set accelerator for the hemihydrate by providing seed crystals that start the crystallization process more quickly. This leads to premature stiffening of the slurry. Thus there is a need in the art for a filler for use in gypsum articles, particularly wallboard, that reduces fuel consumption 10 by replacing calcined gypsum, by reducing the amount of water driven from the set product or both. The filler should have fire retardancy approximately equal to set gypsum and it should be inexpensive, readily available and should not decrease the strength of the finished product. 15 The prior art has failed to adequately address the problem of improving the efficacy of a given polycarboxylate dispersant. Improving the efficacy of a dispersant would reduce the cost of the dispersant and maintaining the reasonable price of gypsum products. 20 Thus, there is a need in the art to reduce the dosage of dispersants used in a gypsum slurry while maintaining flowability of the slurry. Reduction in dispersant use would result in saving of costs spent on the dispersant and would reduce adverse side effects, such as set retardation. 5 WO 2007/027530 PCT/US2006/033297 SUMMARY OF THE INVENTION These and other needs are met or exceeded by the use of the present invention which utilizes an improved, coated landplaster as a filler in gypsum products. The coated landplaster also optionally 5 serves as a delivery vehicle for a modifier that enhances performance of polycarboxylate dispersants. One embodiment of this invention is drawn to a gypsum slurry that includes calcium sulfate hemihydrate, water and calcium sulfate dihydrate coated with a hydrophilic, dispersible coating. The 10 coating is less soluble than the calcium sulfate dihydrate to delay exposure of the landplaster to the remainder of the slurry, preventing premature crystallization and the early stiffening that accompanies it. Another embodiment of this invention is a gypsum slurry that includes calcium sulfate hemihydrate, a polycarboxylate 15 dispersant, water and coated calcium sulfate dihydrate. In this case, the hydrophilic, dispersible coating is selected to serve as a modifier to enhance the ability of the dispersant to fluidize the gypsum slurry. A method of making the slurry includes selecting a coating that is less soluble than calcium sulfate hemihydrate. Calcium 20 sulfate dihydrate is coated with the hydrophilic, dispersible coating, then combined with water and calcium sulfate hemihydrate. Replacement of a portion of the calcined gypsum with coated landplaster results in lower requirements for calcined gypsum, resulting in savings realized from a reduction in fuel and power 25 consumed by the calcining process. Plants that are limited by stucco production may also achieve an increase in capacity since more wallboard can be made with the same amount of stucco. 6 WO 2007/027530 PCT/US2006/033297 Coating of the landplaster reduces its ability to act as a set accelerator. By covering the landplaster crystal, the hemihydrate molecules do not have access to the seed crystals as long as the coating remains in place. As the coating dissolves into the slurry 5 water, the landplaster is exposed and begins to catalyze the hydration reactions. However, removal of the coating takes time that delays initiation of the setting reactions so that premature stiffening of the slurry is minimized or avoided. Another possibility it that the coating is insoluble and merely renders the landplaster inert. The ability to 10 control when the landplaster is available to initiate setting reactions allows reduction the usage of set accelerator, resulting in a cost savings. If the coating is highly dispersible, the landplaster may disperse in the slurry more easily than the calcined gypsum it 15 replaces, allowing a further reduction in the water needed to fluidize the slurry. Less fuel will be required for the kiln where there is less water to dry from the product. Instead of the energy savings, plants that are kiln-limited can realize additional capacity from increased line speeds and sale of additional product. 20 Where there is a capacity increase, it is obtained without a significant increase in capital spending. This capital becomes available for other projects or interest that may have been paid could be saved. Since a large number of plants are limited by either stucco production or by kiln drying, use of this coating could have wide 25 application. In some embodiments, the loss in strength is avoided entirely. Landplaster results in higher strengths than many other fillers. At least one of the preferred coatings results in a product where there is no loss in strength at all. This produces a particularly good 7 product, having many of the properties of gypsum set from 100% calcined gypsum. When used in formulations with polycarboxylate dispersants, the coated landplaster is also usable as a vehicle to deliver a modifier for enhancement of the 5 dispersant. A number of modifiers are known and are suitable for deposition onto the landplaster particle. Definitions of the specific embodiments of the invention as claimed herein follow. According to a first embodiment of the invention, there is provided a 0 gypsum slurry comprising: calcium sulfate hemihydrate; water; and calcium sulfate dihydrate coated with a hydrophilic, dispersible coating selected from at least one of the group consisting of soda ash and hydrated lime, 5 wherein said coating is less soluble than calcium sulfate hemihydrate. According to a second embodiment of the invention, there is provided a method of making a gypsum slurry, comprising: selecting a hydrophilic, dispersible coating that is less soluble than calcium sulfate dehydrate, from at least one of the group consisting of soda ash and .0 hydrated lime; coating calcium sulfate dihydrate with said coating; and combining the coated calcium sulfate dihydrate with calcium sulfate hemihydrate and water to form the slurry. According to a third embodiment of the invention, there is provided a 25 method of making a wallboard panel comprising: selecting a hydrophilic, dispersible coating material that is both less soluble than calcium sulfate dihydrate and enhances the efficacy of a polycarboxylate dispersant, from at least one of the group consisting of soda ash 8 and hydrated lime; coating calcium sulfate dihydrate with said coating material; combining the coated calcium sulfate dihydrate with calcium sulfate hemihydrate, the polycarboxylate dispersant and water to form a slurry; 5 depositing the slurry on a facing material; forming the panel; and allowing the slurry to set. DETAILED DESCRIPTION OF THE INVENTION The gypsum slurry of this invention is made using water, calcined D gypsum and a coated landplaster. Although the benefits of this invention are most clear when used in a slurry that includes a polycarboxylate, it is useful in any embodiment where it is desirable to utilize landplaster as a filler but premature thickening is to be avoided. Any calcined gypsum or stucco is useful in this slurry. Either alpha or 5 beta calcined stucco is useful. Stuccos from a variety of sources can be used, including synthetic gypsum. As discussed below, average or low salt stuccos are preferred in embodiments where polycarboxylate dispersants are used due to possible interaction. Landplaster is used as a filler to replace a portion of the stucco. Since e0 landplaster is already in the dihydrate form, it requires no water of hydration and thus has less of a water demand than stucco. However, landplaster does not participate in the crystal formation reactions, and therefore does not become bound into the crystal matrix to the same degree as the hemihydrate. Some loss in strength occurs, particularly if the amount of landplaster exceeds 10% of the total amount of gypsum 25 materials. Any amount of landplaster [Text continues on page 9.] 8a WO 2007/027530 PCT/US2006/033297 may be used, but preferably, the amount of landplaster is about 3-10% of the total calcium sulfate materials on a dry basis. As used in this application, the term "calcium sulfate materials" includes calcium sulfate in all of its forms, including the anhydrate, hemihydrate and the 5 dihydrate forms. The landplaster is coated with any applicable coating that prevents early onset of thickening of the gypsum slurry. Preferably, the coating is less soluble than the stucco, providing time for mixing and incorporation of other additives before the landplaster is 10 exposed. The coating is applicable to the landplaster in any suitable coating method. Preferably the landplaster is added to a coating solution. Once coated, the landplaster is optionally dried for later use. However, in a preferred coating method, the coating is precipitated onto the landplaster while the landplaster remains slurried with the 15 coating solution. Energy required to dry the landplaster is saved. The coating slurry with the coated landplaster is then incorporated with the stucco slurry before the product is formed. Coated landplaster, water, excess coating and/or byproducts are all added to the stucco slurry prior to final mixing. 20 Many coatings are useful in the present invention. Preferred coatings include DEQUEST particularly DEQUEST 2006, phosphonate dispersants (Solutia, St. Louis, MO) or calcium carbonate. Other coatings made of trisodium phosphate or tetrasodium pyrophosphate are also useful. Any material is usable 25 that is capable of being coated onto the landplaster particles, that is less soluble than the landplaster and reduces the active sites of nucleation. The coating that is particularly useful is calcium carbonate. The coating is preferably formed by precipitation of the 9 WO 2007/027530 PCT/US2006/033297 calcium carbonate onto the calcium sulfate dihydrate, or landplaster, from solution. One embodiment of the coating is obtained by combining hydrated lime, such as calcium magnesium hydroxide, and soda ash or sodium carbonate. Next the calcium sulfate dihydrate is 5 added. A replacement reaction occurs, bringing calcium carbonate together to form a solid. The addition of lime also causes the calcium carbonate to precipitate onto the landplaster specifically, rather than on the interior of the mixer or other equipment. After the coated landplaster has been prepared, the stucco and any other additives are 10 added to the slurry. When 10% by weight of the total calcium sulfate material is in the form of landplaster coated with calcium carbonate and 90% by weight of the calcium sulfate material is in the form of hemihydrate, almost 10% water reduction is achieved compared to 100% hemihydrate. 15 Preferably, the water is warm when the lime and soda ash are added to it. Use of warm water appears to improve the efficacy of the coating process. Water temperatures up to 120'F are especially useful for dissolving the salts, and the use of higher temperatures is contemplated. 20 In some embodiments, reduction in the amount of water used to make the slurry is achieved by the addition of a dispersant, such as a polycarboxylate or naphthalene sulfonate. The dispersant attaches itself to the calcium sulfate, then charged groups on the backbone and the side chains on the branches of the polymer repel 25 each other, causing the gypsum particles to-spread out and flow easily. When the slurry flows more easily, the amount of water can be reduced and still obtain a flowable fluid. In general, reduction in water results in lower drying costs. 10 WO 2007/027530 PCT/US2006/033297 Any polycarboxylate dispersant that is useful for improving fluidity in gypsum is preferred in the slurry of this invention. A number of polycarboxlate dispersants, particularly polycarboxylic ethers, are preferred types of dispersants. One of the preferred class 5 of dispersants used in the slurry includes two repeating units. It is described further in co-pending U.S. Serial No. 11/152,418, entitled "Gypsum Products Utilizing a Two-Repeating Unit System and Process for Making Them", previously incorporated by reference. These dispersants are products of Degussa Construction Polymers, 10 GmbH (Trostberg Germany) and are supplied by Degussa Corp. (Kennesaw, GA) (hereafter "Degussa") and are hereafter referenced as the "PCE2 1-Type Dispersants". The first repeating unit is an olefinic unsaturated mono carboxylic acid repeating unit, an ester or salt thereof, or an olefinic 15 unsaturated sulphuric acid repeating unit or a salt thereof. Preferred first repeating units include acrylic acid or methacrylic acid. Mono- or divalent salts are suitable in place of the hydrogen of the acid group. The hydrogen can also be replaced by hydrocarbon group to form the ester. 20 The second repeating unit satisfies Formula 1, -H2C-CR 2_ 25 [CHO p 0 R 30 and R 1 is derived from an unsaturated (poly)alkylene glycol ether group according to Formula Il. 11 WO 2007/027530 PCT/US2006/033297 -(CmH 2 mO)x (CnH 2 nO)y-(CH 2 CHO)z-R 4
R
3 Referring to Formula I, the alkenyl repeating unit 5 optionally includes a C1 to C3 alkyl group between the polymer backbone and the ether linkage. The value of p is an integer from 0-3, inclusive. Preferably, p is either 0 or 1. R 2 is either a hydrogen atom or an aliphatic C1 to C5 hydrocarbon group, which may be linear, branched, saturated or unsaturated. Examples of preferred repeating 10 units include acrylic acid and methacrylic acid. The polyether group of Formula Il contains multiple C2 C4 alkyl groups, including at least two different alkyl groups, connected by oxygen atoms. M and n are, independently, integers from 2 to 4, inclusive. Preferably, at least one of m and n is 2. X and y are, 15 independently, integers from 55 to 350, inclusive. The value of z is from 0 to 200, inclusive. R 3 is a non-substituted or substituted aryl group and preferably phenyl. R 4 is hydrogen or an aliphatic C1 to C20 hydrocarbon group, a cycloaliphatic C5 to C8 hydrocarbon group, a substituted C6 to C14 aryl group or a group conforming at least one of 20 Formula 111(a), 111(b) and 111(c). o 111(a)
-O-C-R
5 0 0 11116(b) -- O--R -C-OH 1l1(b) 12 WO 2007/027530 PCT/US2006/033297 O H ll 1 7111(c) -O-C-N--R In the above formulas, R 5 and R , independently of each other, represent an alkyl, aryl, aralkyl or alkylaryl group. R 6 is a bivalent alkyl, aryl, aralkyl or alkylaryl group. A particularly useful dispersant of the PCE211-Type Dispersants is designated PCE211 5 (hereafter "211"). Other polymers in this series known to be useful in wallboard include PCE111. PCE21 1-Type dispersants are described more fully in U.S. Serial No. 11/152,678, filed June 14, 2005, and a continuation-in-part of U.S. Serial No. 11/152,678, filed June, 2006 by Degussa Construction Polymers, both entitled "Polyether-Containing 10 Copolymer", and herein incorporated by reference. The molecular weight of the PCE21 I Type dispersant is preferably from about 20,000 to about 60,000 Daltons. Surprisingly, it has been found that the higher molecular weight dispersants cause less retardation of set time than dispersants having a molecular weight 15 greater than 60,000 Daltons. Generally longer side chain length, which results in an increase in overall molecular weight, provides better dispersibility. However, tests with gypsum indicate that efficacy of the dispersant is reduced at molecular weights above 50,000 Daltons. 20 The first repeating unit preferably makes up from about 30% to about 99 mole % of the total repeating units, more preferably from about 40 to about 80%. From about I to about 70 mole % of the repeating units are the second repeating unit, more preferably from about 10 to about 60 mole %. 25 Another class of polycarboxylate compounds that are useful in this invention is disclosed in U.S. Patent No. 6,777,517, 13 WO 2007/027530 PCT/US2006/033297 herein incorporated by reference and hereafter referenced as the "2641-Type Dispersant". Preferably, the dispersant includes at least three repeating units shown in Formula IV(a), IV(b) and IV(c).
-CH
2
~CR
3 2 IV(a)
LCH
2 ] p--OCmH 2 mO n--R 2 R 4 -CH-C- IV(b) I I S T
-CH
2 -CR-- IV(c) 5 In this case, both acrylic and maleic acid repeating units are present, yielding a higher ratio of acid groups to vinyl ether groups.
R
1 represents a hydrogen atom or an aliphatic hydrocarbon radical having from 1 to 20 carbon atoms. X represents OM, where M is a hydrogen atom, a monovalent metal cation, an ammonium ion or an 10 organic amine radical. R 2 can be hydrogen, an aliphatic hydrocarbon radical having from 1 to 20 carbon atoms, a cycloaliphatic hydrocarbon radical having from 6 to 14 carbon atoms, which may be substituted.
R
3 is hydrogen or an aliphatic hydrocarbon radical having from 1 to 5 carbon atoms, which are optionally linear or branched, saturated or 15 unsaturated. R 4 is hydrogen or a methyl group, depending on whether the structural units are acrylic or methacrylic. P can be from 0 to 3. M is an integer from 2 to 4, inclusive, and n is an integer from 0 to 200, inclusive. PCE21I-Type and 2641-Type dispersants are manufactured by Degussa Construction Polymers, GmbH (Tr6stberg, 20 Germany) and marketed in the United States by Degussa Corp. 14 WO 2007/027530 PCT/US2006/033297 (Kennesaw, GA). Preferred 2641-Type Dispersants are sold by Degussa as MELFLUX 2641 F, MELFLUX 2651F and MELFLUX 2500L dispersants. 2641-Type dispersants (MELFLUX is a registered trademark of Degussa Construction Polymers, GmbH) are described 5 for use in wallboard and gypsum slurries in U.S. Serial No. 11/152,661, entitled "Fast Drying Wallboard", previously incorporated by reference. Yet another preferred dispersant family is sold by Degussa and referenced as "1641-Type Dispersants". This dispersant 10 is more fully described in U.S. Patent No. 5,798,425, herein incorporated by reference. A particularly preferred 1641-Type Dispersant is shown in Formula VI and marketed as MELFLUX 1641F dispersant by Degussa. This dispersant is made primarily of two repeating units, one a vinyl ether and the other a vinyl ester. In 15 Formula V, m and n are the mole ratios of the component repeating units, which can be randomly positioned along the polymer chain. CH-CH m CH 2 CH nV O=C C=0 0 Na*--O 0 H 2
CH
2 CH 2
CH
2 0 q O p H
CH
3 These dispersants are particularly well-suited for use 20 with gypsum. While not wishing to be bound by theory, it is believed that the acid repeating units bind to the hemihydrate crystals while the long polyether chains of the second repeating unit perform the 15 WO 2007/027530 PCT/US2006/033297 dispersing function. Since it is less retardive than other dispersants, it is less disruptive to the manufacturing process of gypsum products such as wallboard. The dispersant is used in any effective amount. To a large extent, the amount of dispersant selected is dependant on 5 the desired fluidity of the slurry. As the amount of water decreases, more dispersant is required to maintain a constant slurry fluidity. Since polycarboxylate dispersants are relatively expensive components, it is preferred to use a small dose, preferably less than 2% or more preferably less than I % by weight based on the weight of 10 the dry calcium sulfate material. Preferably, the dispersant is used in amounts of about 0.05% to about 0.5% based on the dry weight of the calcium sulfate material. More preferably, the dispersant is used in amounts of about 0.01% to about 0.2% on the same basis. In measuring a liquid dispersant, only the polymer solids are considered 15 in calculating the dosage of the dispersant, and the water from the dispersant is considered when a water/stucco ratio is calculated. Many polymers can be made with the same repeating units using different distributions of them. The ratio of the acid containing repeating units to the polyether-containing repeating unit is 20 directly related to the charge density. Preferably, the charge density of the co-polymer is in the range of about 300 to about 3000 pequiv. charges/g co-polymer. It has been found that the most effective dispersant tested for water reduction in this class of dispersants, MELFLUX 2651 F, has the highest charge density. 25 However, it has also been discovered that the increase in charge density further results in an increase in the retardive effect of the dispersant. Dispersants with a low charge density, such as MELFLUX 2500L, retard the set times less than the MELFLUX 2651 F dispersant that has a high charge density. Since retardation in set 16 WO 2007/027530 PCT/US2006/033297 times increases with the increase in efficacy obtained with dispersants of high charge density, making a slurry with low water, good flowability and reasonable set times requires keeping of the charge density in a mid-range. More preferably, the charge density of the co-polymer is in 5 the range of about 600 to about 2000 pequiv. charges/g co-polymer. Modifiers are optionally added to a gypsum slurry to enhance performance of a polycarboxylate dispersant. The modifier can be any substance, liquid or solid, which when combined with a polycarboxylate dispersant in a gypsum slurry, leads to an 10 improvement the efficacy of the dispersant. Modifiers are not intended to be dispersants in themselves, but serve to allow the dispersant to be more effective. For example, at constant concentrations of dispersant, better fluidity is obtained when the modifier is used compared to the same slurry without the modifier. 15 Although the exact chemistry involved in the use of modifiers is not fully understood, at least two different mechanisms are responsible for the increase in dispersant efficacy. Lime, for example, reacts with the polycarboxylate in the aqueous solution to uncoil the dispersant molecule. In contrast, soda ash reacts on the gypsum 20 surface to help improve the dispersant effect. Any mechanism can be used by the modifier to improve the efficacy of the dispersant for the purposes of this invention. Theoretically, if the two mechanisms work independently, combinations of modifiers can be found that utilize the full effect of both mechanisms and result in even better dispersant 25 efficacy. Preferred modifiers include cement, lime, also known as quicklime or calcium oxide, slaked lime, also known as calcium hydroxide, soda ash, also known as sodium carbonate, potassium carbonate, also known as potash, and other carbonates, silicates, 17 WO 2007/027530 PCT/US2006/033297 hydroxides, phosphonates and phosphates. Preferred carbonates include sodium and potassium carbonate. Sodium silicate is a preferred silicate. When lime or slaked lime is used as the modifier, it is 5 used in concentrations of about 0.15% to about 1.0% based on the weight of the dry calcium sulfate material. In the presence of water, lime is quickly converted to calcium hydroxide, or slaked lime, and the pH of the slurry becomes alkaline. The sharp rise in pH can cause a number of changes in the slurry chemistry. Certain additives, 10 including trimetaphosphate, break down as the pH increases. There can also be problems with hydration and, where the slurry is used to make wallboard or gypsum panels, there are problems with paper bond at high pH. For workers who come in contact with the slurry, strongly alkaline compositions can be irritating to the skin and contact 15 should be avoided. Above pH of about 11.5, lime no longer causes an increase in fluidity. Therefore, it is preferred in some applications to hold the pH below about nine for maximum performance from this modifier. In other applications, such as flooring, a high pH has the benefit of minimizing mold and mildew. Alkali metal hydroxides, 20 especially sodium and potassium hydroxides are preferred for use in flooring. Other preferred modifiers include carbonates, phosphonates, phosphates and silicates. Preferably, the modifiers are used in amounts less than 0.25% based on the weight of the dry -25 calcium sulfate material. Above these concentrations, increases in the amount of modifier causes a decrease in the dispersant efficacy. These modifiers are preferably used in amounts of from about 0.05 to about 0.2 weight %. 18 WO 2007/027530 PCT/US2006/033297 Many of the modifiers disclosed above are advantageously applied as the landplaster coating. In such cases, the coated landplaster serves two functions, that of reducing premature thickening of the slurry, as well as a delivery vehicle for the modifier. 5 Water demand of the slurry is reduced by permitting use of a dihydrate filler, as well as delivering the modifier that enhances the efficacy of the dispersant. The resulting slurry utilizes water very efficiently. The charge density of the dispersant has also been found to affect the ability of the modifier to interact with the dispersant. 10 Given a family of dispersants with the same repeating units, the modifier causes a greater increase in efficacy in the dispersant having the higher charge density. It is important to note that although the general trend is to obtain a higher efficacy boost with higher charge density, when comparing the effectiveness of dispersants having 15 different repeating units, the effectiveness of the dispersants may be considerably different at the same charge density. Thus, adjustment of the charge density may not be able to overcome poor fluidity with a particular family of dispersants for that application. It has also been noted that the reaction of the 20 polycarboxylate dispersants and the modifiers react differently when used in different gypsum media. While not wishing to be bound by theory, the impurities present in gypsum are believed to contribute to the efficacy of both the dispersant and the modifier. Among the impurities present in stucco are salts that vary by geographical 25. - location. Many salts are known -to be set accelerators or set retarders. These same salts may also change the efficacy of the polycarboxylate dispersant by affecting the degree of fluidity that can be achieved. Some preferred polycarboxylates, including the PCE21 1-Type Dispersants, are best utilized with a low salt stucco. Other 19 WO 2007/027530 PCT/US2006/033297 dispersants, such as the 2641-Type Dispersants are suitable for use with high-salt stuccos. As a result of the use of fluidity enhancing dispersants and modifiers to boost their performance, the amount of water used to 5 fluidize the slurry can be reduced compared to slurries made without these additives. It must be understood that the stucco source, the calcining technique, the dispersant family, the charge density and the modifier all work together to produce a slurry of a given fluidity. In the laboratory, it is possible to reduce the water level close to, equal to, or 10 even below that theoretically required to fully hydrate the calcium sulfate hemihydrate. When used in a commercial setting, process considerations may not allow water reduction to this degree. When used to make gypsum board, a number of additives are useful to improve the properties of the finished article. 15 Traditional amounts of additives are used. Amounts of several additives are reported as "lbs/MSF," which stands for pounds of additive per one thousand square feet of board. Some embodiments of the invention employ a foaming agent to yield voids in the set gypsum-containing product to provide 20 lighter weight. In these embodiments, any of the conventional foaming agents known to be useful in preparing foamed set gypsum products can be employed. Many such foaming agents are well known and readily available commercially, e.g. the HYONIC line of soaps from GEO Specialty Chemicals, Ambler, PA. Foams and a preferred 25 method for preparing foamed gypsum products are disclosed in U.S. Patent No. 5,683,635, herein incorporated by reference. Dispersants are used to improve the flowability of the slurry and reduce the amount of water used to make the slurry. Any known dispersant is useful, including polycarboxylates, sulfonated 20 WO 2007/027530 PCT/US2006/033297 melamines or naphthalene sulfonate. Naphthalene sulfonate is another preferred dispersant, and is used in amounts of about 0 lb/MSF to 18 lb/MSF (78.5 g/m 2 ), preferably from about 4 lb/MSF (17.5 g/m 2 ) to about 12 lb/MSF (52.4 g/m 2 ). A preferred naphthalene 5 sulfonate dispersant is DAXAD Dispersant (Dow Chemical, Midland, MI). Even where dispersants are used in the coating, it maybe advantageous to have additional dispersant to further improve the fluidity of the slurry. A trimetaphosphate compound is added to the gypsum 10 slurry in some embodiments to enhance the strength of the product and to improve sag resistance of the set gypsum. Preferably the concentration of the trimetaphosphate compound is from about 0.07% to about 2.0% based on the weight of the calcium sulfate material. Gypsum compositions including trimetaphosphate compounds are 15 disclosed in U.S. Patent No. 6,342,284 and 6,632,550, both herein incorporated by reference. Exemplary trimetaphosphate salts include sodium, potassium or lithium salts of trimetaphosphate, such as those available from Astaris, LLC., St. Louis, MO. Care must be exercised when using trimetaphosphate with lime or other modifiers that raise 20 the pH of the slurry. Above a pH of about 9.5, the trimetaphosphate loses its ability to strengthen the product and the slurry becomes severely retardive. Other additives are also added to the slurry as are typical for the particular application to which the gypsum slurry will be put. 25 Set retarders (up to about 2 lb./MSF-(9.8g/m2)) or dry accelerators (up to about 35 lb./MSF (170 g/m2)) are added to modify the rate at which the hydration reactions take place. "CSA" is a set accelerator comprising 95% calcium sulfate dihydrate co-ground with 5% sugar and heated to 250*F (121*C) to caramelize the sugar. CSA is 21 WO 2007/027530 PCT/US2006/033297 available from USG Corporation, Southard, OK plant, and is made according to U.S. Patent No. 3,573,947, herein incorporated by reference. Potassium sulfate is another preferred accelerator. HRA is calcium sulfate dihydrate freshly ground with sugar at a ratio of about 5 5 to 25 pounds (2.2 to 11.4 kg) of sugar per 100 pounds (4.5 kg) of calcium sulfate material. It is further described in U.S. Patent No. 2,078,199, herein incorporated by reference. Both of these are preferred accelerators. Another accelerator, known as wet gypsum accelerator 10 or WGA, is also a preferred accelerator. A description of the use of and a method for making wet gypsum accelerator are disclosed in U.S. Patent No. 6,409,825, herein incorporated by reference. This accelerator includes at least one additive selected from the group consisting of an organic phosphonic compound, a phosphate 15 containing compound or mixtures thereof. This particular accelerator exhibits substantial longevity and maintains its effectiveness over time such that the wet gypsum accelerator can be made, stored, and even transported over long distances prior to use. The wet gypsum accelerator is used in amounts ranging from about 5 to about 80 20 pounds per thousand square feet (24.3 to 390 g/m 2 ) of board product. Other potential additives to the wallboard are biocides to reduce growth of mold, mildew or fungi. Depending on the biocide selected and the intended use for the wallboard, the biocide can be added to the covering, the gypsum core or both. Examples of biocides 25 include boric acid, pyrithione salts and copper salts. -Biocides can be added to either the covering or the gypsum core. When used, biocides are used in the coverings in amounts of less than 500 ppm. Pyrithione is known by several names, including 2-mercaptopyridine N-oxide; 2-pyridinethiol-1-oxide (CAS Registry No. 1121-31-9); 1 22 WO 2007/027530 PCT/US2006/033297 hydroxypyridine-2-thione and 1 hydroxy-2(IH)-pyridinethione (CAS Registry No. 1121-30-8). The sodium derivative (C 5
H
4 NOSNa), known as sodium pyrithione (CAS Registry No. 3811-73-2), is-one embodiment of this salt that is particularly useful. Pyrithione salts are 5 commercially available from Arch Chemicals, Inc. of Norwalk, CT, such as Sodium OMADINE or Zinc OMADINE. In addition, the gypsum composition optionally can include a starch, such as a pregelatinized starch or an acid-modified starch. Starches are used in amounts of from about 3 to about 20 lbs/ 10 MSF (14.6 to 97.6 g/m 2 ) to increase paper bond and strengthen product. The inclusion of the pregelatinized starch increases the strength of the set and dried gypsum cast and minimizes or avoids the risk of paper delamination under conditions of increased moisture (e.g., with regard to elevated ratios of water to calcined gypsum). One 15 of ordinary skill in the art will appreciate methods of pregelatinizing raw starch, such as, for example, cooking raw starch in water at temperatures of at least about 185 0 F (85 0 C) or other methods. Suitable examples of pregelatinized starch include, but are not limited to, PCF 1000 Starch, commercially available from Lauhoff Grain 20 Company and AMERIKOR 818 and HQM PREGEL starches, both commercially available from Archer Daniels Midland Company (Decatur, IL). If included, the pregelatinized starch is present in any suitable amount. For example, if included, the pregelatinized starch can be added to the mixture used to form the set gypsum composition 25 such that it is present in an amount of from about 0.5% to about 10% percent by weight of the set gypsum composition. Starches such as USG95 (United States Gypsum Company, Chicago, IL) are also optionally added for core strength. 23 WO 2007/027530 PCT/US2006/033297 Other known additives may be used as needed to modify specific properties of the product. Sugars, such as dextrose, are used to improve the paper bond at the ends of the boards. Wax emulsions or siloxanes are used for water resistance. If stiffness is needed, boric 5 acid is commonly added. Fire retardancy can be improved by the addition of vermiculite. These and other known additives are useful in the present slurry and wallboard formulations. Glass fibers are optionally added to the slurry in amounts of up to 11 lb./MSF (54 g/m 2 ). Up to 15 lb./MSF (73.2 g/m 2 ) of paper fibers are also added to 10 the slurry. Wax emulsions are added to the gypsum slurry in amounts up to 90 lb./MSF (0.439 kg/m 2 ) to improve the water-resistency of the finished gypsum board panel. 24 WO 2007/027530 PCT/US2006/033297 EXAMPLE 1 A number of coatings were added to landplaster and tested in the laboratory for their ability to improve the fluidity of the 5 samples. Components and amounts used in each sample are shown in Table 1. Forty grams of landplaster and water as shown were added to a Hobart Model N-50 mixer followed by addition of the additive. The mixer was turned on low (setting 1) for five minutes. 10 The amount of dispersant was sufficient to yield 0.6 grams of solids. The dispersant was weighed out on a small plastic boat and added to the mixture by hand. Three hundred sixty grams of stucco was then added to the mixer and allowed to soak for 15 seconds. The slurry was mixed on medium speed (setting 2) for 15 seconds. 15 TABLE I Dispersant Water, Additive Amt., Patty Stiff Vicat grams grams Size, cm Time Set 211 200 Control 0.0 22.8 2:55 9:00 211 200 DEQUEST 0.80 28.0 22:00 >30:00 211 200 SodaAsh 0.80 26.5 2:35 7:50 211 200 Lime 0.80 26.5 3:15 10:20 Daxad 240 Control 0.0 18.8 2:55 9:00 Daxad 240 DEQUEST 0.80 26.0 12:00 23:00 Daxad 240 SodaAsh 0.80 12.2 <1:30 7:00 Daxad 240 Lime 0.80 17.5 2:30 7:10 25 WO 2007/027530 PCT/US2006/033297 For testing, a portion of the slurry was transferred to a Slump Cylinder 2 inches (5 cm) in diameter and four inches (10 cm) tall and a 7 ounce (207 cc) cup. Contents of the cylinder were screeded flush with the top of the cylinder. If compression strength 5 and temperature rise set measurements were taken, additional slurry was poured into brass two inch cube molds and an insulated cup. Sixty seconds from the start of the stucco soak, the slump cylinder was raised with a pneumatic mechanism. The diameter of the resultant patty was measured in at least two directions and recorded 10 as the average of the two readings. "Stiffening time" is measured as the elapsed time from the beginning of the stucco soak to when a Vicat needle drawn through the slurry left a definite line that did not flow back. The stiffening time is a measure of the hydration of the slurry. "Vicat set" refers to the elapsed time from the onset of the 15 stucco soak until a 300 gram Vicat needle positioned at the surface of the 7 ounce cup fails to penetrate to the bottom of the sample. As shown in the data above, the addition of DEQUEST 2006 and Soda Ash each resulted in an increase in fluidity of the slurry as indicated by the increase in patty size over the control sample. 20 DEQUEST 2006 increased patty size with both 211 (polycarboxylate) and Daxad (naphthalene sulfonate) dispersants. EXAMPLE 2 -25 Additional laboratory tests were conducted where accelerator was added to reduce the retardive effects of the dispersant. The slurry was made more similar to a wallboard slurry by the addition of foam. 26 One hundred twenty grams of landplaster and water as shown were added to a Hobart Model N-50 mixer followed by addition of the additive. The mixer was turned on low (setting 1) for five minutes. The amount of dispersant was enough to give 1.8 grams of solids. The dispersant was weighed out on a small plastic boat 5 and added to the mixture by hand. One thousand eighty grams of stucco were then added to the mixer and allowed to soak for 15 seconds. The slurry was mixed on medium speed (setting 2) for 15 seconds. TABLE 11 Dispersant Water, Additive Amt., Patty Size, Stiff Time grams grams cm 211 600 Control 0.0 20.7 2:15 211 600 DEQUEST 0.60 25.5 2:50 211 600 TSP 0.60 22.5 2:30 211 600 TSPP 0.60 25.0 2:40 Daxad 720 Control 0.0 13.2 <1:50 Daxad 720 DEQUEST 0.60 17.1 1:45 Daxad 720 TSP 0.60 14.0 1:20 Daxad 720 TSPP 0.60 15.2 2:10 10 Other dry additives, such as set accelerators or starches, are preferably combined with the stucco prior to entry to the slurry. Wet additives are generally added directly to the mixer prior to introduction of the dry components. When all components are added, the resulting slurry is mixed until a homogeneous slurry is obtained. 15 The term "comprise" and variants of the term such as "comprises" or '"comprising" are used herein to denote the inclusion of a stated integer or stated integers but not to exclude any other integer or any other integers, unless in the context or usage an exclusive interpretation of the term is required. 27 Any reference to publications cited in this specification is not an admission that the disclosures constitute common general knowledge in Australia 28

Claims (17)

1. A gypsum slurry comprising: calcium sulfate hemihydrate; water; and 5 calcium sulfate dihydrate coated with a hydrophilic, dispersible coating selected from at least one of the group consisting of soda ash and hydrated lime, wherein said coating is less soluble than calcium sulfate hemihydrate.
2. The slurry of claim 1 wherein the temperature of said water is greater than 1000F. 0
3. The slurry of claim 1 or claim 2, wherein said coating is applied at a rate of up to 0.2% based on the total dry weight of calcium sulfate.
4. The slurry of any one of claims 1 to 3, wherein said coated calcium sulfate dihydrate is present in amounts of up to about 10% by weight based on the combined weight of said calcium sulfate hemihydrate and said calcium sulfate dihydrate.
5 5. The slurry of any one of claims 1 to 4 further comprising a polycarboxylate dispersant.
6. The slurry of claim 5, wherein said coating comprises a modifier that enhances the efficacy of the dispersant.
7. A method of making a gypsum slurry, comprising: 20 selecting a hydrophilic, dispersible coating that is less soluble than calcium sulfate dehydrate, from at least one of the group consisting of soda ash and hydrated lime; coating calcium sulfate dihydrate with said coating; and combining the coated calcium sulfate dihydrate with calcium sulfate 25 hemihydrate and water to form the slurry.
8. The method of claim 7, wherein said combining step comprises mixing.
9. The method of claim 7 or claim 8, wherein said coating step comprises precipitating, spraying or dipping.
10. The method of any one of claims 7 to 9 further comprising adding a 29 polycarboxylate dispersant to the slurry.
11. The method of claim 10, wherein said coating comprises a modifier for enhancing performance of said dispersant.
12. A method of making a wallboard panel comprising: 5 selecting a hydrophilic, dispersible coating material that is both less soluble than calcium sulfate dihydrate and enhances the efficacy of a polycarboxylate dispersant, from at least one of the group consisting of soda ash and hydrated lime; coating calcium sulfate dihydrate with said coating material; combining the coated calcium sulfate dihydrate with calcium sulfate 0 hemihydrate, the polycarboxylate dispersant and water to form a slurry; depositing the slurry on a facing material; forming the panel; and allowing the slurry to set.
13. The method of claim 12, wherein said coating material is applied in amounts of 5 up to 0.2% based on the combined dry weight of the calcium sulfate hemihydrate and calcium sulfate dihydrate.
14. The method of claim 12 or claim 13, wherein the calcium sulfate dihydrate comprises from about 3% to about 10% of the combined weight of the calcium sulfate dihydrate and the calcium sulfate hemihydrate. '0
15. A gypsum slurry as defined in claim 1 and substantially as herein described with reference to the section entitled 'Detailed Description of the Invention'.
16. A method of making a gypsum slurry as defined in claim 7 and substantially as herein described with reference to the section entitled 'Detailed Description of the Invention'. 25
17. A method of making a wall board panel as defined in claim 12 and substantially as herein described with reference to the section entitled 'Detailed Description of the Invention'. Date: 9 August 2010 30
AU2006285062A 2005-08-31 2006-08-25 Modified landplaster as a wallboard filler Ceased AU2006285062B2 (en)