JP3156150B2 - Olefin-based decorative sheet with weather resistance - Google Patents

Olefin-based decorative sheet with weather resistance

Info

Publication number
JP3156150B2
JP3156150B2 JP15287896A JP15287896A JP3156150B2 JP 3156150 B2 JP3156150 B2 JP 3156150B2 JP 15287896 A JP15287896 A JP 15287896A JP 15287896 A JP15287896 A JP 15287896A JP 3156150 B2 JP3156150 B2 JP 3156150B2
Authority
JP
Japan
Prior art keywords
layer
resin
decorative sheet
olefin
sheet
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Expired - Fee Related
Application number
JP15287896A
Other languages
Japanese (ja)
Other versions
JPH09314791A (en
Inventor
晴男 大野
義昭 根津
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Dai Nippon Printing Co Ltd
Original Assignee
Dai Nippon Printing Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Family has litigation
First worldwide family litigation filed litigation Critical https://patents.darts-ip.com/?family=15550104&utm_source=google_patent&utm_medium=platform_link&utm_campaign=public_patent_search&patent=JP3156150(B2) "Global patent litigation dataset” by Darts-ip is licensed under a Creative Commons Attribution 4.0 International License.
Application filed by Dai Nippon Printing Co Ltd filed Critical Dai Nippon Printing Co Ltd
Priority to JP15287896A priority Critical patent/JP3156150B2/en
Publication of JPH09314791A publication Critical patent/JPH09314791A/en
Application granted granted Critical
Publication of JP3156150B2 publication Critical patent/JP3156150B2/en
Anticipated expiration legal-status Critical
Expired - Fee Related legal-status Critical Current

Description

【発明の詳細な説明】DETAILED DESCRIPTION OF THE INVENTION

【0001】[0001]

【発明の属する技術分野】本発明は、住宅の外装及び内
装材、或いは家具、家電製品等の化粧材として用いられ
る化粧シートに関する。特に、塩化ビニル樹脂シートを
使用せず且つ耐候性に優れた化粧シートに関する。
BACKGROUND OF THE INVENTION 1. Field of the Invention The present invention relates to a decorative sheet used as an exterior and interior material of a house, or a decorative material for furniture, home electric appliances and the like. In particular, it relates to a decorative sheet that does not use a vinyl chloride resin sheet and has excellent weather resistance.

【0002】[0002]

【従来の技術】従来、住宅の外装用、内装用等の各種化
粧材として、塩化ビニル樹脂シートを用いた化粧シート
が多用されている。塩化ビニル樹脂製のシートは、Vカ
ットや熱エンボス加工等の加工適性、印刷やラミネート
に対する接着性、さらに耐候性にも優れる上に、コスト
的にも安価であり、全体としてバランス良く極めて優秀
な性能を有するからである。ところが、近年、地球環境
問題が重要視される様になり、化粧シート材としての塩
化ビニル樹脂の代替材料が希求されている。それは、家
屋、家具、家電製品等の廃材を焼却処分する際に、塩酸
ガスが発生するからである。そこで、塩化ビニル樹脂の
代替材料として、ポリオレフィン系樹脂を用いた化粧シ
ートが各種試みられている。例えば、特開平6−798
30号公報で提案された技術は、ポリオレフィン系樹脂
のエンボスの再現性向上を試みるものであり、特開平6
−79850号公報ではエンボスに更にワイピング加工
を試みた化粧シートが提案されている。
2. Description of the Related Art A decorative sheet using a vinyl chloride resin sheet has been frequently used as a decorative material for exterior and interior of a house. The sheet made of vinyl chloride resin is excellent in processability such as V-cut and hot embossing, adhesion to printing and lamination, and weather resistance, and is inexpensive in terms of cost. This is because it has performance. However, in recent years, global environmental issues have become increasingly important, and there has been a demand for alternative materials to vinyl chloride resins as decorative sheet materials. This is because hydrochloric acid gas is generated when incinerating waste materials such as houses, furniture, and home electric appliances. Therefore, various kinds of decorative sheets using a polyolefin resin as an alternative material to the vinyl chloride resin have been tried. For example, JP-A-6-798
The technique proposed in Japanese Patent Publication No. 30 attempts to improve the reproducibility of emboss of a polyolefin resin.
Japanese Patent Application Laid-Open No. 79850/1999 proposes a decorative sheet in which wiping is further attempted on embossing.

【0003】[0003]

【発明が解決しようとする課題】しかしながら、耐候性
の問題は、ポリオレフィン系樹脂単体では劣り、従来の
塩化ビニル樹脂製化粧シート並の性能を得ることはでき
ない。そこで、各種紫外線吸収剤等の耐候性を向上させ
る耐候性向上剤をポリオレフィン系樹脂に添加する事が
試みられているが、化粧シートとした場合の耐候性の点
で満足すべき充分な性能は未だ得られていない。特に印
刷絵柄層や着色隠蔽層に、塩化ビニル−酢酸ビニル共重
合体、塩素化ポリプロピレン等をビヒクルの樹脂成分と
する、従来から塩化ビニル樹脂製化粧シートに多用され
ているインクを用いた場合には、ポリオレフィン系樹脂
の耐候性向上剤としてヒンダードアミン系光安定剤を添
加したものでも、充分な耐候性能は得られなかった。
However, the problem of weather resistance is inferior to a polyolefin resin alone, and it cannot achieve the same performance as a conventional vinyl chloride resin decorative sheet. Therefore, it has been attempted to add a weather resistance improver such as various ultraviolet absorbers to improve the weather resistance to the polyolefin resin. Not yet obtained. In particular, when using an ink that has been frequently used for a decorative sheet made of a vinyl chloride resin, using a vinyl chloride-vinyl acetate copolymer, a chlorinated polypropylene, or the like as a resin component of the vehicle for the printed pattern layer or the colored concealing layer. However, even when a hindered amine light stabilizer was added as a weather resistance improver for a polyolefin resin, sufficient weather resistance was not obtained.

【0004】[0004]

【課題を解決するための手段】そこで、上記課題を解決
するために、本発明の化粧シートでは、表側より順に透
明オレフィン系樹脂層、印刷絵柄層、着色隠蔽層よりな
る構成において、透明オレフィン系樹脂層にヒンダード
アミン系光安定剤等の光安定剤を含有させ、且つ印刷絵
柄層及び着色隠蔽層に、塩素を含まない樹脂を用いる構
成とした。また、表側より順に透明オレフィン系樹脂
層、印刷絵柄層、着色オレフィン系樹脂層よりなる構成
の化粧シートにおいても、透明オレフィン系樹脂層にヒ
ンダードアミン系光安定剤等の光安定剤を含有させ、且
つ印刷絵柄層に塩素を含まない樹脂を用いる構成とし
た。この結果、印刷絵柄層や着色隠蔽層の成分樹脂とし
て従来多用していた、塩素化ポリプロピレンや塩化ビニ
ル−酢酸ビニル共重合体等の塩素含有樹脂の塩素成分に
よる光安定剤への悪影響を無くした。
Therefore, in order to solve the above-mentioned problems, the decorative sheet of the present invention comprises a transparent olefin resin layer, a printed pattern layer, and a colored concealment layer in order from the front side. A light stabilizer such as a hindered amine light stabilizer is contained in the resin layer, and a resin containing no chlorine is used for the printed picture layer and the colored concealing layer. Also, in order from the front side, a transparent olefin-based resin layer, a printed pattern layer, and a decorative sheet having a configuration including a colored olefin-based resin layer, the transparent olefin-based resin layer contains a light stabilizer such as a hindered amine-based light stabilizer, and The printed pattern layer is made of a resin containing no chlorine. As a result, the adverse effect on the light stabilizer due to the chlorine component of the chlorine-containing resin such as chlorinated polypropylene or vinyl chloride-vinyl acetate copolymer, which has been frequently used as a component resin of the print pattern layer or the color hiding layer, has been eliminated. .

【0005】[0005]

【発明の実施の形態】以下、本発明の透明オレフィン系
化粧シートを説明する。図1は本発明の透明オレフィン
系化粧シートの一形態として、オレフィン系樹脂層が単
層の場合を示す断面図である。また、図2は本発明の透
明オレフィン系化粧シートの他の形態として、オレフィ
ン系樹脂層が2層の場合を示す断面図である。図におい
て、1は、透明オレフィン系樹脂層、2は印刷絵柄層、
3は着色隠蔽層、4は着色オレフィン系樹脂層である。
図1の単層仕様の化粧シート10は、透明オレフィン系
樹脂層1として樹脂シートを用い、この裏面側に印刷絵
柄層2を印刷し、さらに着色隠蔽層3を印刷又は塗工形
成すれば得ることができる。また、図2の2層仕様の化
粧シート20は、例えば、着色オレフィン系樹脂層4上
に印刷絵柄層2を印刷後、この上から樹脂シートを熱ラ
ミネーション又はドライラミネーションにより積層する
か、樹脂をTダイにより溶融押出しと同時に積層して透
明オレフィン系樹脂層1として積層すれば得ることがで
きる。或いは、逆に、透明オレフィン系樹脂層の裏面に
印刷絵柄層を形成後に、熱ラミネーション又はドライラ
ミネーションにより着色したオレフィン系樹脂シートを
積層するか、着色したオレフィン系樹脂をTダイにより
溶融押出しと同時に積層しても得ることができる。
BEST MODE FOR CARRYING OUT THE INVENTION Hereinafter, a transparent olefin decorative sheet of the present invention will be described. FIG. 1 is a cross-sectional view showing a case where the olefin-based resin layer is a single layer as one embodiment of the transparent olefin-based decorative sheet of the present invention. FIG. 2 is a cross-sectional view showing another embodiment of the transparent olefin-based decorative sheet of the present invention in which the number of olefin-based resin layers is two. In the figure, 1 is a transparent olefin resin layer, 2 is a printed picture layer,
3 is a colored concealing layer, and 4 is a colored olefin-based resin layer.
1 is obtained by using a resin sheet as the transparent olefin-based resin layer 1, printing the printed picture layer 2 on the back surface thereof, and further printing or coating the colored concealing layer 3. be able to. In addition, the decorative sheet 20 of the two-layer specification in FIG. 2 is, for example, after printing the printed picture layer 2 on the colored olefin-based resin layer 4, laminating the resin sheet from above by heat lamination or dry lamination, It can be obtained by laminating at the same time as melt extrusion with a T-die and laminating as a transparent olefin-based resin layer 1. Alternatively, conversely, after forming a printed pattern layer on the back surface of the transparent olefin-based resin layer, an olefin-based resin sheet colored by heat lamination or dry lamination may be laminated, or the colored olefin-based resin may be melt-extruded with a T-die and simultaneously. It can also be obtained by lamination.

【0006】透明オレフィン系樹脂層 透明オレフィン系樹脂層1としては、ポリエチレン、ポ
リプロピレン、エチレン−プロピレン共重合体、エチレ
ン−ブテン−1共重合体、プロピレン−ブテン−1共重
合体、ポリブテン−1、ブテン−1・プロピレン・エチ
レン三元共重合体、ブテン−1・ヘキセン−1・オクテ
ン−1三元共重合体、ポリメチルペンテン、エチレン−
酢酸ビニル共重合体、エチレン−ビニルアルコール共重
合体、或いはポリエチレン−アクリル酸共重合体等によ
るエチレン系アイオノマー等の樹脂が使用できる。な
お、この透明オレフィン系樹脂層の樹脂としては、塩素
化ポリプロピレンの様に分子中に塩素原子を含有しない
オレフィン系樹脂を用いる。また、柔軟性、加工性を向
上させる目的で、上記樹脂にエラストマー成分を併用し
ても良い。エラストマー成分としては、ポリオレフィン
系熱可塑性エラストマー(TPO)、スチレン系熱可塑
性エラストマー、ポリエステル系熱可塑性エラストマー
等の熱可塑性エラストマーが挙げられる。なお、この
内、ポリオレフィン系熱可塑性エラストマーは、単独で
も透明オレフィン系樹脂層として使用できる。
[0006] As a transparent olefin resin layer transparent olefin resin layer 1, polyethylene, polypropylene, ethylene - propylene copolymer, ethylene - butene-1 copolymer, propylene - butene-1 copolymer, polybutene-1, Butene-1, propylene, ethylene terpolymer, butene-1, hexene-1, octene-1 terpolymer, polymethylpentene, ethylene
Resins such as an ethylene ionomer such as a vinyl acetate copolymer, an ethylene-vinyl alcohol copolymer, or a polyethylene-acrylic acid copolymer can be used. As the resin of the transparent olefin resin layer, an olefin resin containing no chlorine atom in the molecule, such as chlorinated polypropylene, is used. For the purpose of improving flexibility and processability, an elastomer component may be used in combination with the above resin. Examples of the elastomer component include thermoplastic elastomers such as polyolefin-based thermoplastic elastomer (TPO), styrene-based thermoplastic elastomer, and polyester-based thermoplastic elastomer. Of these, the polyolefin-based thermoplastic elastomer can be used alone as a transparent olefin-based resin layer.

【0007】単層仕様の化粧シートにおいては、透明オ
レフィン系樹脂層は、Tダイ法、カレンダ法等により成
膜して樹脂シートの形態から得ることができる。この場
合、延伸或いは未延伸のいずれも樹脂シートでも用いる
ことができるが、Vカット加工適性等の成形適性の点で
は未延伸の樹脂シートの方が好ましい。なお、単層仕様
の場合、この上に印刷する印刷絵柄層の密着性向上のた
めに、コロナ処理又はプライマー処理を施しても良い。
ちなみに、図3に示す化粧シートは、プライマー層5を
透明オレフィン系樹脂層となる樹脂シートに施してから
印刷絵柄層2、着色隠蔽層3を形成した構成例を示すも
のである。また、透明オレフィン系樹脂層1は、図2の
2層仕様では、樹脂シートの積層による方法以外にも、
前記した如く、印刷絵柄層形成済みの着色オレフィン系
樹脂シートに、溶融押出しと同時に積層する方法等でも
形成することができる。
In a single-layer decorative sheet, the transparent olefin-based resin layer can be obtained in the form of a resin sheet by forming a film by a T-die method, a calendar method or the like. In this case, either a stretched or unstretched resin sheet can be used, but an unstretched resin sheet is more preferable in terms of formability such as suitability for V-cut processing. In the case of a single-layer specification, a corona treatment or a primer treatment may be performed to improve the adhesion of a printed picture layer printed thereon.
Incidentally, the decorative sheet shown in FIG. 3 shows a configuration example in which the primer layer 5 is applied to a resin sheet to be a transparent olefin-based resin layer, and then the printed picture layer 2 and the colored concealing layer 3 are formed. The transparent olefin-based resin layer 1 has a two-layer structure shown in FIG.
As described above, it can also be formed by a method of laminating simultaneously with melt extrusion on a colored olefin-based resin sheet on which a printed picture layer has been formed.

【0008】なお、透明オレフィン系樹脂層1の厚さ
は、単層仕様の場合には、印刷や塗工を施す樹脂シート
として取り扱うので、25〜500μm、望ましくは5
0〜150μmの範囲に通常は設定する。薄すぎると強
度が低下し印刷機や塗工機での搬送が困難となる。ま
た、2層仕様の場合の透明オレフィン系樹脂層1の厚さ
は、化粧シート製造において樹脂シートとして取り扱う
ならば、上記範囲とするが、着色オレフィン系樹脂層側
を樹脂シートとして取り扱い、溶融押出し法やカレンダ
ー法で透明オレフィン系樹脂層を積層と同時に成膜する
のであれば、上記下限値よりも薄くすることも可能であ
る。但し、表面側となる透明オレフィン系樹脂層には、
耐候性向上剤を含有させることから、薄くしすぎると耐
候性が低下するので、せいぜい10μm以上、好ましく
は20μm以上とする。
The thickness of the transparent olefin-based resin layer 1 is 25 to 500 μm, preferably 5 to 500 μm in the case of a single-layer specification, because the thickness is handled as a resin sheet to be printed or coated.
Usually, it is set in the range of 0 to 150 μm. If it is too thin, the strength will decrease and it will be difficult to convey it in a printing machine or a coating machine. The thickness of the transparent olefin resin layer 1 in the case of the two-layer specification is within the above range if it is handled as a resin sheet in the production of a decorative sheet, but the colored olefin resin layer side is treated as a resin sheet and melt-extruded. If the transparent olefin-based resin layer is formed simultaneously with the lamination by a method or a calendar method, the thickness can be made smaller than the lower limit. However, the transparent olefin resin layer on the surface side has
Since the weather resistance improver is contained, if the thickness is too small, the weather resistance is reduced. Therefore, the thickness is at most 10 μm or more, preferably 20 μm or more.

【0009】透明オレフィン系樹脂層には耐候性向上の
為に耐候性向上剤として光安定剤を含有させることが必
要である。光安定剤はヒンダードアミン系光安定剤が好
ましい。ヒンダードアミン系光安定剤は、テトラアルキ
ルピペリジンを母核に持ち、紫外線で発生するラジカル
を補足するラジカル補足作用がある他、ヒドロペルオキ
シド(ROOH)の不活性作用等の各種作用機構により
その効果が発揮されると推定されており、多機能の安定
剤として優れた性能が得られる。ヒンダードアミン系光
安定剤の具体例としては、例えば、ビス−(2,2,
6,6−テトラメチル−4−ピペリジル)セバケート、
ビス−(N−メチル−2,2,6,6−テトラメチル−
4−ピペリジル)セバーケート、ビス−(1,2,2,
6,6−ペンタメチル−4−ピペリジル)セバケート、
1,2,2,6,6−ペンタメチル−4−ピペリジル−
トリデシル−1,2,3,4,−ブタンテトラカルボキ
シレート、テトラギス−(2,2,6,6−テトラメチ
ル−4−ピペリジル)−1,2,3,4−ブタンテトラ
カルボキシレート等が挙げられ、その他、例えば特公平
4−82625号公報に開示されている化合物などのヒ
ンダードアミン系ラジカル捕捉剤が挙げられる。ヒンダ
ードアミン系光安定剤の含有量は、樹脂全量に対して
0.1〜3重量%の範囲が好ましい。これより少ない
と、耐候性向上効果が充分に得られず、又これより多い
と着色化し、多量に入れても効果的に変化がなく好まし
くない。
It is necessary for the transparent olefin-based resin layer to contain a light stabilizer as a weather resistance improver in order to improve weather resistance. The light stabilizer is preferably a hindered amine light stabilizer. The hindered amine light stabilizer has a tetraalkylpiperidine in its mother nucleus, has a radical scavenging action to scavenge radicals generated by ultraviolet rays, and exerts its effect by various action mechanisms such as an inactive action of hydroperoxide (ROOH). Thus, excellent performance can be obtained as a multifunctional stabilizer. Specific examples of the hindered amine light stabilizer include, for example, bis- (2,2,
6,6-tetramethyl-4-piperidyl) sebacate,
Bis- (N-methyl-2,2,6,6-tetramethyl-
4-piperidyl) sebercate, bis- (1,2,2,2)
6,6-pentamethyl-4-piperidyl) sebacate,
1,2,2,6,6-pentamethyl-4-piperidyl-
Tridecyl-1,2,3,4-butanetetracarboxylate, tetragis- (2,2,6,6-tetramethyl-4-piperidyl) -1,2,3,4-butanetetracarboxylate and the like. And hindered amine radical scavengers such as the compounds disclosed in Japanese Patent Publication No. 4-82625. The content of the hindered amine light stabilizer is preferably in the range of 0.1 to 3% by weight based on the total amount of the resin. If the amount is less than this, the effect of improving the weather resistance cannot be sufficiently obtained, and if it is more than this, coloring occurs, and even if it is contained in a large amount, there is no effective change, which is not preferable.

【0010】また、透明オレフィン系樹脂層には耐候性
向上の為に上記光安定剤を含有させる以外に、従来公知
の紫外線吸収剤を耐候性向上剤として併用することもで
きる。併用により耐候性はより向上する。紫外線吸収剤
としては、具体的には、例えば、有機系の化合物として
は、2−(2′−ヒドロキシ−3′,5′−ジ−ter
t−ブチルフェニル)−5−クロロベンゾトリアゾー
ル、2−(2′−ヒドロキシ−3′−tert−ブチル
−5′−メチルフェニル)−5−クロロベンゾトリアゾ
ール、2−(2′−ヒドロキシ−3′−tert−アミ
ル−5′−イソブチルフェニル)−5−クロロベンゾト
リアゾール、2−(2′−ヒドロキシ−3′−イソブチ
ル−5′−メチルフェニル)−5−クロロベンゾトリア
ゾール、2−(2′−ヒドロキシ−3′−イソブチル−
5′−プロピルフェニル)−5−クロロベンゾトリアゾ
ール等の2′−ヒドロキシフェニル−5−クロロベンゾ
トリアゾール系紫外線吸収剤類、2−(2′−ヒドロキ
シ−3′,5′−ジ−tert−ブチルフェニル)ベン
ゾトリアゾール、2−(2′−ヒドロキシ−5′−メチ
ルフェニル)ベンゾトリアゾール等の2′−ヒドロキシ
フェニルベンゾトリアゾール系紫外線吸収剤類、2,
2′−ジヒドロキシ−4−メトキシベンゾフェノン、
2,2′−ジヒドロキシ−4,4′−ジメトキシベンゾ
フェノン、2,2′,4,4′−テトラヒドロキシベン
ゾフェノン等の2,2′−ジヒドロキシベンゾフェノン
系紫外線吸収剤類、2−ヒドロキシ−4−メトキシベン
ゾフェノン、2,4−ジヒドロキシベンゾフェノン等の
2−ヒドロキシベンゾフェノン系紫外線吸収剤類、サリ
チル酸フェニル、4−t−ブチル−フェニル−サリシレ
ート等のサリチル酸エステル系紫外線吸収剤類、2−エ
チル−ヘキシル−2−シアノ−3,3−ジフェニルアク
リレート、エチル−2−シアノ−3,3−ジフェニルア
クリレート、オクチル−2−シアノ−3,3−ジフェニ
ルアクリレート等のシアノアクリレート系紫外線吸収剤
類等が挙げられる。また、無機系の化合物としては粒径
1μm以下、可視光線透明度の点でより好ましくは0.
2μm以下の酸化亜鉛、酸化鉄、酸化チタン、酸化セリ
ウム等の無機酸化物の紫外線吸収剤類等が挙げられる。
In addition to the above-mentioned light stabilizer for improving the weather resistance, a conventionally known ultraviolet absorber may be used as a weather resistance improver in the transparent olefin resin layer. The combined use improves the weather resistance. As the ultraviolet absorber, specifically, for example, as an organic compound, 2- (2'-hydroxy-3 ', 5'-di-ter
t-butylphenyl) -5-chlorobenzotriazole, 2- (2'-hydroxy-3'-tert-butyl-5'-methylphenyl) -5-chlorobenzotriazole, 2- (2'-hydroxy-3 '-Tert-amyl-5'-isobutylphenyl) -5-chlorobenzotriazole, 2- (2'-hydroxy-3'-isobutyl-5'-methylphenyl) -5-chlorobenzotriazole, 2- (2'- Hydroxy-3'-isobutyl-
2'-hydroxyphenyl-5-chlorobenzotriazole-based ultraviolet absorbers such as 5'-propylphenyl) -5-chlorobenzotriazole, 2- (2'-hydroxy-3 ', 5'-di-tert-butyl) 2′-hydroxyphenylbenzotriazole-based ultraviolet absorbers such as phenyl) benzotriazole and 2- (2′-hydroxy-5′-methylphenyl) benzotriazole;
2'-dihydroxy-4-methoxybenzophenone,
2,2'-dihydroxybenzophenone-based ultraviolet absorbers such as 2,2'-dihydroxy-4,4'-dimethoxybenzophenone and 2,2 ', 4,4'-tetrahydroxybenzophenone; 2-hydroxy-4-methoxy 2-hydroxybenzophenone UV absorbers such as benzophenone and 2,4-dihydroxybenzophenone; salicylate UV absorbers such as phenyl salicylate and 4-tert-butyl-phenyl-salicylate; 2-ethyl-hexyl-2- Examples include cyanoacrylate-based ultraviolet absorbers such as cyano-3,3-diphenylacrylate, ethyl-2-cyano-3,3-diphenylacrylate, and octyl-2-cyano-3,3-diphenylacrylate. Further, as the inorganic compound, the particle diameter is preferably 1 μm or less, and more preferably 0.1 μm from the viewpoint of visible light transparency.
UV absorbers of inorganic oxides such as zinc oxide, iron oxide, titanium oxide, cerium oxide and the like having a size of 2 μm or less.

【0011】また、透明オレフィン系樹脂層には、上記
した耐候性を向上させる成分を含有させる以外に、さら
に適宜、難燃性を付与する為に、水酸化アルミニウム、
水酸化マグシウム、三酸化アンチモン等の難燃剤、或い
は炭酸カルシウム等の無機充填剤を含有させても良い。
難燃剤の含有量は、目的とする難燃グレードにより適宜
調整するが、樹脂100重量部に対して10〜100重
量部程度である。また、透明オレフィン系樹脂層は、透
明であれば顔料、染料等の色材により着色されていても
良い。
In addition to the above-mentioned components for improving the weather resistance, the transparent olefin-based resin layer further contains aluminum hydroxide,
A flame retardant such as magnesium hydroxide and antimony trioxide or an inorganic filler such as calcium carbonate may be contained.
The content of the flame retardant is appropriately adjusted depending on the intended flame retardant grade, but is about 10 to 100 parts by weight based on 100 parts by weight of the resin. The transparent olefin-based resin layer may be colored with a coloring material such as a pigment or a dye as long as it is transparent.

【0012】印刷絵柄層 印刷絵柄層2としては、必須成分としてヒンダードアミ
ン系光安定剤等の光安定剤を含有する上記透明オレフィ
ン系樹脂層1に接する為に、塩素を含有しない化合物で
構成する。従って、従来、塩化ビニル樹脂シートの化粧
シートで用いられていた、塩化ビニル−酢酸ビニル共重
合体、塩素化ポリプロピレン等の分子中に塩素原子を含
有する樹脂は用いない。これら塩素含有樹脂等の化合物
は、紫外線による脱塩酸反応で生じた塩酸が透明オレフ
ィン系樹脂層に達し、そこに存在するヒンダードアミン
系の光安定剤を失活させ又その光安定化作用を阻害する
ので、所望の満足すべき耐候性が得られなくなる。この
ため、印刷絵柄層を構成する樹脂成分としては、インク
化可能で塩素を含有しない樹脂であればいずれでも良
く、熱可塑性樹脂、或いは、熱硬化性樹脂、電離放射線
硬化性樹脂等の硬化性樹脂等の従来公知の各種樹脂を使
用できる。
Printing Pattern Layer The printing pattern layer 2 is made of a chlorine-free compound so as to be in contact with the transparent olefin resin layer 1 containing a light stabilizer such as a hindered amine light stabilizer as an essential component. Therefore, a resin containing a chlorine atom in a molecule, such as a vinyl chloride-vinyl acetate copolymer and a chlorinated polypropylene, which has been conventionally used for a decorative sheet of a vinyl chloride resin sheet, is not used. In these compounds such as chlorine-containing resins, the hydrochloric acid generated by the dehydrochlorination reaction by ultraviolet rays reaches the transparent olefin-based resin layer, deactivates the hindered amine-based light stabilizer present therein, or inhibits its light-stabilizing action. Therefore, the desired satisfactory weather resistance cannot be obtained. For this reason, any resin component that can be made into an ink and does not contain chlorine may be used as the resin component constituting the print pattern layer, and may be a curable resin such as a thermoplastic resin, a thermosetting resin, or an ionizing radiation-curable resin. Conventionally known various resins such as resins can be used.

【0013】上記熱可塑性樹脂としては、アクリル樹
脂、ウレタン樹脂、ポリエステル樹脂、ポリアミド樹
脂、酢酸ビニル樹脂、セルロース樹脂、ブチラール樹脂
等の各種の塩素非含有の熱可塑性樹脂が挙げられる。ま
た、熱硬化性樹脂としては、ポリエステルポリオール、
ポリアクリルポリオール、ポリエーテルポリオール等と
イソシアネート化合物とを反応させる2液硬化型インキ
として用いるポリウレタン樹脂、ポリアミドやポリアミ
ン等で硬化させるエポキシ樹脂、重合触媒で硬化させる
不飽和ポリエステル樹脂、或いは、酸で硬化させる、メ
ラミン樹脂、尿素樹脂、アルキド樹脂等が挙げられる。
また、電離放射線硬化性樹脂としては、分子中にエチレ
ン性不飽和結合を有する、プレポリマー又はオリゴマ
ー、及び希釈モノマー等からなる樹脂組成物が使用でき
る。プレポリマー又はオリゴマーとしては、不飽和ポリ
エステル、ポリエステルアクリレート、ウレタンアクリ
レート、エポキシアクリレート、ポリエーテルアクリレ
ート等が挙げられる。また希釈モノマーとしては単官
能、多官能の、低粘度で揮発性が少なく皮膚刺激性の少
ないものが好ましくは用いられる。なお、印刷絵柄層を
構成する塩素非含有の樹脂としては、上記の熱可塑性樹
脂、熱硬化性樹脂、電離放射線硬化性樹脂の樹脂を2種
類以上を併用することもある。
Examples of the thermoplastic resin include various chlorine-free thermoplastic resins such as acrylic resin, urethane resin, polyester resin, polyamide resin, vinyl acetate resin, cellulose resin, and butyral resin. Further, as the thermosetting resin, polyester polyol,
Polyurethane resin used as a two-component curable ink for reacting polyacryl polyol, polyether polyol, etc. with an isocyanate compound, epoxy resin cured with polyamide, polyamine, etc., unsaturated polyester resin cured with a polymerization catalyst, or cured with acid Melamine resin, urea resin, alkyd resin and the like.
Further, as the ionizing radiation-curable resin, a resin composition comprising a prepolymer or oligomer having an ethylenically unsaturated bond in a molecule, a diluting monomer, or the like can be used. Examples of the prepolymer or oligomer include unsaturated polyester, polyester acrylate, urethane acrylate, epoxy acrylate, and polyether acrylate. As the diluent monomer, a monofunctional or polyfunctional monomer having low viscosity, low volatility and low skin irritation is preferably used. As the chlorine-free resin constituting the printed picture layer, two or more of the above-mentioned thermoplastic resins, thermosetting resins and ionizing radiation-curable resins may be used in combination.

【0014】印刷絵柄層は、ビヒクルに上記の塩素非含
有の樹脂を用いたインクを、グラビア印刷、オフセット
印刷、凸版印刷、フレキソ印刷、シルクスクリーン印刷
等の公知の印刷法によって形成することができる。イン
ク中の着色剤としては、従来公知の顔料、染料等の色材
のいずれも使用できるが、特に耐候性の点では、例え
ば、ベンガラ、二酸化チタン、朱、群青、緑青(塩基性
炭酸銅)、カーボンブラック等の無機質顔料や、アゾ顔
料、フタロシアニン顔料、キナクリドン系顔料やイソイ
ンドリノン系顔料等の縮合多環状顔料等の有機質顔料等
が、優れた特性を発揮する。顔料としては光輝性顔料で
も良く、また、必要に応じて適宜、炭酸カルシウム、シ
リカ、アルミナ、硫酸バリウム等の体質顔料等も使用で
きる。なお、印刷絵柄層を形成するためのインクは、溶
剤系、水系いずれでも良く、またそれぞれの系におい
て、溶解系、分散系のいずれでも良い。
The printed picture layer can be formed by using a known ink such as gravure printing, offset printing, letterpress printing, flexographic printing, silk screen printing, etc., using the above-mentioned chlorine-free resin as a vehicle. . As the colorant in the ink, any of conventionally known coloring materials such as pigments and dyes can be used. In particular, in terms of weather resistance, for example, red iron oxide, titanium dioxide, vermilion, ultramarine, patina (basic copper carbonate) In addition, inorganic pigments such as carbon black, and organic pigments such as azo pigments, phthalocyanine pigments, and condensed polycyclic pigments such as quinacridone pigments and isoindolinone pigments exhibit excellent properties. As the pigment, a brilliant pigment may be used, and if necessary, extender pigments such as calcium carbonate, silica, alumina, barium sulfate and the like may be used. The ink for forming the print pattern layer may be any of a solvent-based ink and an aqueous-based ink, and in each system, may be any of a dissolved system and a dispersed system.

【0015】着色隠蔽層 着色隠蔽層3は、化粧シートが適用される表面を隠蔽す
る為に全面に形成されるものであり、上記印刷絵柄層2
で挙げた樹脂と同様の樹脂を使用することができる。た
だし、着色隠蔽層は、化粧シート使用時に被着体に接着
剤に面する層であり、その用途で用いられる接着剤に対
する接着性を考慮した樹脂を選定する。また、着色剤等
の顔料も同様であるが、隠蔽顔料として更に、例えば酸
化チタン、酸化亜鉛等の隠蔽性に優れた顔料を樹脂10
0重量部に対し50〜300重量部配合することが多
い。なお、着色隠蔽層は通常は不透明とするが、用途に
よっては着色剤を用いて隠蔽顔料配合量は減らして隠蔽
性を減じ透明着色とすることもある。着色隠蔽層は印刷
絵柄層同様に印刷法で形成しても良いが、塗工法でも形
成することができる。塗工法としては、グラビアコー
ト、ロールコート、リバースコート、ドクターコート等
の従来公知の各種塗工手段が利用できる。塗布量は乾燥
時で2〜30g/m2 の範囲が望ましい。少な過ぎると
隠蔽力が低下する。また、多すぎても隠蔽力は飽和して
意味がない。
The colored concealing layer colored concealing layer 3 is intended to be formed on the entire surface in order to conceal the surface of the decorative sheet is applied, the printed pattern layer 2
The same resins as those mentioned in the above can be used. However, the colored concealing layer is a layer facing the adhesive on the adherend when the decorative sheet is used, and a resin is selected in consideration of the adhesiveness to the adhesive used in the application. The same applies to pigments such as coloring agents. However, as the concealing pigment, a pigment having excellent concealing properties, such as titanium oxide and zinc oxide, may be used as a resin 10.
In many cases, 50 to 300 parts by weight is added to 0 part by weight. The colored concealing layer is usually made opaque, but depending on the application, a coloring agent may be used to reduce the amount of the concealing pigment to reduce the concealing property, thereby providing a transparent coloring. The colored concealing layer may be formed by a printing method like the printed picture layer, but can also be formed by a coating method. As a coating method, various conventionally known coating means such as a gravure coat, a roll coat, a reverse coat, and a doctor coat can be used. The coating amount is desirably in the range of 2 to 30 g / m 2 when dried. If the amount is too small, the hiding power decreases. Also, if the amount is too large, the hiding power is saturated and is meaningless.

【0016】着色オレフィン系樹脂層 着色オレフィン系樹脂層4に用いられ得る樹脂として
は、前記した透明オレフィン系樹脂層用の樹脂が挙げら
れる。ただ、着色オフレィン系樹脂層の場合は、上記着
色隠蔽層同様に下地の隠蔽性が要求されるので、酸化チ
タン、酸化亜鉛等の隠蔽顔料を含有させ、適宜着色顔料
などの着色剤と併用する。なお、着色オレフィン系樹脂
層は通常は不透明とするが、用途によっては着色剤を用
いて隠蔽顔料配合量は減らし透明着色としても良い。ま
た、透明オレフィン系樹脂層同様に難燃剤等を含有させ
ても良い。着色オレフィン系樹脂層4は、着色樹脂シー
トとして成膜したものによるのが一般的であるが、前述
した如く、透明オレフィン系樹脂層に印刷絵柄層を形成
後に、その上から溶融押出しにより成膜と同時に積層す
ることでも形成できる。
Colored olefin-based resin layer Examples of the resin that can be used in the colored olefin-based resin layer 4 include the resins for the transparent olefin-based resin layer described above. However, in the case of a colored off-line resin layer, since the underlying layer is required to be concealed as in the case of the colored concealed layer, a concealing pigment such as titanium oxide or zinc oxide is contained, and is appropriately used in combination with a coloring agent such as a colored pigment. . The colored olefin-based resin layer is usually opaque, but depending on the application, a coloring agent may be used to reduce the blending amount of the concealing pigment to achieve transparent coloring. Further, like the transparent olefin-based resin layer, a flame retardant or the like may be contained. The colored olefin-based resin layer 4 is generally formed by forming a film as a colored resin sheet. However, as described above, after forming a printed pattern layer on the transparent olefin-based resin layer, the film is formed by melt extrusion from above. At the same time, it can be formed by stacking.

【0017】プライマー層 図3及び図4にプライマー層5を設けた構成例の化粧シ
ートを例示する。プライマー層5は適宜、層間密着力向
上の為に設ける。例えば、単層仕様においては、印刷絵
柄層や着色隠蔽層が施される透明オレフィン系樹脂シー
トに施される。また、2層仕様においては、印刷絵柄層
が施される着色オレフィン系樹脂シート、或いは透明オ
レフィン系樹脂シート、或いはこれら樹脂シートのラミ
ネート用として、いずれか一方又は両方のシートに設け
る。本発明の化粧シートで、プライマー層の樹脂として
も、塩素非含有の樹脂を用いることが好ましい。塩素含
有樹脂でも、(印刷絵柄層や着色隠蔽層を塩素非含有と
した事による)一定の耐候性向上効果は得られるが、顕
著な効果は期待できない。特にトップクリヤー層となる
透明オレフィン系樹脂層に接するプライマー層には、塩
素非含有の樹脂を用いるべきである。プライマー層に用
いる塩素を含有しない樹脂としては、前述した絵柄印刷
層で列挙した、熱可塑性樹脂、熱硬化性樹脂や電離放射
線硬化性樹脂等の硬化性樹脂を用いることができる。な
お、プライマー層の形成は適宜コロナ処理を施した面に
従来公知の塗工法、印刷法で行えば良いが、必要に応じ
て塗工適性、印刷適性等を考慮して各種の充填剤、添加
剤を適宜含有させる。
Primer Layer FIGS. 3 and 4 show examples of a decorative sheet provided with a primer layer 5. The primer layer 5 is appropriately provided for improving interlayer adhesion. For example, in the case of a single-layer specification, it is applied to a transparent olefin-based resin sheet to which a printed picture layer and a colored concealing layer are applied. In the two-layer specification, a colored olefin-based resin sheet or a transparent olefin-based resin sheet on which a printed picture layer is to be provided, or one or both of these sheets is used for laminating these resin sheets. In the decorative sheet of the present invention, it is preferable to use a chlorine-free resin also as the resin of the primer layer. Even with a chlorine-containing resin, a certain effect of improving the weather resistance (by making the printed picture layer and the color hiding layer non-chlorine-containing) can be obtained, but no remarkable effect can be expected. Particularly, a chlorine-free resin should be used for the primer layer in contact with the transparent olefin-based resin layer serving as the top clear layer. As the chlorine-free resin used for the primer layer, curable resins such as thermoplastic resins, thermosetting resins, and ionizing radiation-curable resins listed in the above-described pattern printing layer can be used. The formation of the primer layer may be performed by a conventionally known coating method or printing method on the surface that has been appropriately subjected to corona treatment.However, if necessary, various fillers and additives may be added in consideration of coating suitability, printing suitability, and the like. Agent is appropriately contained.

【0018】なお、本発明の化粧シートでは、透明オレ
フィン系樹脂層の表面に、エンボス加工、サンドブラス
ト加工、ヘアライン加工等により、凹凸形状からなる凹
凸模様を形成しても良い。エンボス加工は、熱プレス方
式の枚葉又は輪転式エンボス機を用いて、例えば印刷絵
柄層等を形成後の、単層シート又は2層仕様に積層され
たシートに対して、その表面にエンボス版を押圧して版
の凹凸形状を賦形することにより凹凸模様を形成する。
エンボス加工のにより形成する凹凸模様としては、木目
導管柄、木目木肌、石材表面凹凸、布帛の表面テクスチ
ュア、梨地、砂目、ヘアライン等でも良く、またこれら
の組み合わせでも良い。さらに、透明オレフィン系樹脂
層表面に形成した凹凸模様の凹部には、必要に応じて公
知の、ドクタブレード法、ロールコート法等によるワイ
ピング加工により着色インクを充填しても良い。着色イ
ンクとしては、印刷絵柄層同様に、ウレタン樹脂、アク
リル樹脂、ポリエステル樹脂等の塩素を含有しない樹脂
が好ましい。なかでもウレタン樹脂となる2液硬化型イ
ンクは密着性、耐溶剤性等が良好で好ましい。また、印
刷絵柄層以外にの絵柄層として、アルミニウム等の部分
金属蒸着層があってもよい。また、この部分金属蒸着層
や絵柄印刷層は転写印刷で形成しても良い。
In the decorative sheet of the present invention, an uneven pattern having an uneven shape may be formed on the surface of the transparent olefin-based resin layer by embossing, sandblasting, hairline processing, or the like. The embossing is performed by using a hot-press type sheet-fed or rotary embossing machine, for example, after forming a printed pattern layer or the like, a single-layer sheet or a sheet laminated in a two-layer specification, and an embossing plate on its surface. Is pressed to shape the uneven shape of the plate to form an uneven pattern.
The concavo-convex pattern formed by embossing may be a wood grain conduit pattern, a wood grain texture, a stone surface unevenness, a fabric surface texture, a satin finish, a grain, a hairline, or a combination thereof. Further, the concave portions of the concavo-convex pattern formed on the surface of the transparent olefin-based resin layer may be filled with a coloring ink by a known wiping process using a doctor blade method, a roll coating method, or the like, if necessary. As the coloring ink, a resin containing no chlorine, such as a urethane resin, an acrylic resin, or a polyester resin, is preferable as in the case of the printed picture layer. Among them, a two-component curable ink that is a urethane resin is preferable because of good adhesion, solvent resistance, and the like. Further, as a picture layer other than the printed picture layer, there may be a partial metal deposition layer of aluminum or the like. The partial metal deposition layer and the pattern printing layer may be formed by transfer printing.

【0019】なお、本発明の化粧シートの用途として
は、各種部材の表面に積層し表面化粧する用途がある。
被接着部としては、鉄、アルミニウム等の金属板、木材
単板、木材合板、木質繊維板等の木質板、ガラス、陶磁
器等のセラミックス、ALC等のセメント板等の板材、
ポリプロピレン、フェノール樹脂等の樹脂板の板材、或
いこれら各種材料からなる、樹脂成形等の立体形状物品
が挙げられる。また、これら各種部材への化粧シートの
積層方法としては、例えば、接着剤層を介して板状部
材に加圧ローラで加圧して積層する方法、特公昭50
−19132号公報等に記載の様に、化粧シートの表面
側となる面をキャビティ側に向く様にして、雌雄両金型
間に配置して樹脂を射出成形する、所謂、射出成形同時
ラミネート法、特公昭56−45768号公報、特公
昭60−58014号公報等に記載の様に、成形品等の
立体形状物品の表面に化粧シートを、間に接着剤層を介
して対向又は載置し、立体形状物品側から真空吸引によ
る圧力差により化粧シートを成形品表面に積層する、所
謂、真空プレス積層法、特公昭61−5895号公報
に記載の様に、円柱、多角柱等の柱状部材の長軸方向
に、化粧シートを間に接着剤層を介して供給しつつ、複
数の向きの異なるローラにより、柱状部材を構成する複
数の側面に順次化粧シートを加圧接着して積層してゆ
く、所謂、ラッピング加工法、実公大15−3112
2号公報、特開昭48−47972号公報等に記載の様
に、先ず化粧シートを板状部材に接着剤層を介して積層
し、次いで板状部材の化粧シートとは反対側の面に、化
粧シートと板状部材との界面に達する、断面がV字状又
はU字状の溝を切削し、次いで該溝内に接着剤を塗布
後、該溝で折り曲げて箱体又は柱状体を形成する、所
謂、Vカット又はUカット加工法、等がある。そして、
これらの方法により化粧シートを積層し表面化粧された
化粧部材は、壁面、天井等の建築内装用装飾材、窓枠、
扉、手摺等の建具類の表面装飾材、家具の表面装飾材、
弱電・OA機器のキャビネット、或いは自動車等の車両
内装材の表面装飾材として用いられ得る。
As a use of the decorative sheet of the present invention, there is a use in which the decorative sheet is laminated on the surface of various members to make the surface decorative.
Examples of the parts to be bonded include iron, metal plates such as aluminum, wood veneer, wood plywood, wood plates such as wood fiber plates, glass, ceramics such as ceramics, and plate materials such as cement plates such as ALC,
Examples include plate materials of resin plates such as polypropylene and phenolic resin, and three-dimensional articles made of these various materials, such as resin molding. Examples of a method of laminating a decorative sheet on these various members include, for example, a method of laminating a plate-like member by pressing with a pressure roller via an adhesive layer,
As described in Japanese Patent Application Laid-Open No. 19132, etc., a so-called simultaneous injection molding lamination method in which resin is injection-molded by disposing the resin between the male and female molds so that the surface on the surface side of the decorative sheet faces the cavity side. As described in JP-B-56-45768 and JP-B-60-58014, a decorative sheet is opposed to or placed on the surface of a three-dimensional article such as a molded article with an adhesive layer interposed therebetween. A decorative sheet is laminated on the surface of a molded article by a pressure difference caused by vacuum suction from the three-dimensional article side, a so-called vacuum press laminating method, as described in JP-B-61-5895, columnar members such as cylinders and polygonal columns. In the long-axis direction, while supplying the decorative sheet through an adhesive layer therebetween, the decorative sheets are sequentially pressure-adhered and laminated on a plurality of side surfaces constituting the columnar member by a plurality of rollers having different directions. So-called wrapping , Jitsuoyakedai 15-3112
No. 2, JP-A-48-47972, etc., first, a decorative sheet is laminated on a plate-like member via an adhesive layer, and then the decorative sheet is placed on the surface of the plate-like member on the side opposite to the decorative sheet. , Cut a V-shaped or U-shaped groove reaching the interface between the decorative sheet and the plate-shaped member, and then apply an adhesive in the groove, and then bend the box to form a box or column. For example, there is a so-called V-cut or U-cut processing method. And
Cosmetic sheets laminated by these methods and decoratively decorated are surface decoration materials for building interiors such as walls, ceilings, window frames,
Surface decoration materials for doors, handrails and other fittings, furniture surface decoration materials,
It can be used as a cabinet for light electric / OA equipment or as a surface decoration material for vehicle interior materials such as automobiles.

【0020】[0020]

【実施例】次に実施例及び比較例により本発明の化粧シ
ートを更に具体的に説明する。なお、文中にて「部」と
あるのは特に断りの無い限り重量基準である。
Next, the decorative sheet of the present invention will be described more specifically with reference to examples and comparative examples. In the following description, “parts” is based on weight unless otherwise specified.

【0021】《実施例1》透明オレフィン系樹脂層とし
て、ポリオレフィン系熱可塑性エラストマー(TPO)
(出光石油化学(株)製、E−2900)100部に対
し、光安定剤としてヒンダードアミン系光安定剤(旭電
化工業(株)製、〔型番〕LA−63)を0.5部配合
したものをTダイから溶融押出しして、0.1mm厚の
透明樹脂シートを作製し、印刷面側をコロナ処理した。
次いで、コロナ処理面に、2液硬化型ウレタン系樹脂に
よるメジウムインク(昭和インク工業(株)製、AFS
メジウム)でプライマー層を、その上に、2液硬化型ウ
レタン系樹脂による柄インク(昭和インク工業(株)
製、AFS)、同じく2液硬化型ウレタン系樹脂による
隠蔽インク(昭和インク工業(株)製、AFS白)で、
印刷絵柄層、着色隠蔽層を順次、グラビア印刷により形
成して、本発明の化粧シートを得た。
Example 1 A polyolefin-based thermoplastic elastomer (TPO) was used as a transparent olefin-based resin layer.
As a light stabilizer, 0.5 part of a hindered amine-based light stabilizer (manufactured by Asahi Denka Kogyo KK, [model number] LA-63) was added to 100 parts of (E-2900, manufactured by Idemitsu Petrochemical Co., Ltd.). The product was melt-extruded from a T-die to produce a 0.1 mm thick transparent resin sheet, and the printed surface side was corona treated.
Next, a medium ink made of a two-component curable urethane resin (AFS manufactured by Showa Ink Industry Co., Ltd., AFS
Media) and a two-component curable urethane resin pattern ink (Showa Ink Industries Co., Ltd.)
AFS), a two-part curable urethane-based concealing ink (AFS White, manufactured by Showa Ink Industries, Ltd.)
A printed pattern layer and a colored concealing layer were sequentially formed by gravure printing to obtain a decorative sheet of the present invention.

【0022】《比較例1》実施例1において、プライマ
ー層形成用インクを、塩化ビニル−酢酸ビニル共重合体
によるインク(大日本インキ化学工業(株)製、ディッ
クシール A−100Z)に代え、且つ印刷絵柄層及び
着色隠蔽層の形成に用いたインクも、どちらも塩化ビニ
ル−酢酸ビニル共重合体とアクリル樹脂とを用いた、柄
インク(昭和インク工業(株)製、化X)及び隠蔽イン
ク(昭和インク工業(株)製、化XNo.7)に代えた
他は、実施例1と同様にして化粧シートを得た。
Comparative Example 1 In Example 1, the ink for forming a primer layer was replaced with an ink made of a vinyl chloride-vinyl acetate copolymer (Dick Seal A-100Z, manufactured by Dainippon Ink and Chemicals, Inc.). In addition, the ink used for forming the print pattern layer and the colored concealing layer is also a pattern ink (manufactured by Showa Ink Industry Co., Ltd., Chemical X) and a concealment, both using a vinyl chloride-vinyl acetate copolymer and an acrylic resin. A decorative sheet was obtained in the same manner as in Example 1 except that the ink was replaced with an ink (manufactured by Showa Ink Industries, Ltd., Chemical X No. 7).

【0023】《比較例2》比較例1において、プライマ
ー層形成用のインクを実施例1で用いたものに代えた他
は、実施例1と同様にして化粧シートを得た。
Comparative Example 2 A decorative sheet was obtained in the same manner as in Example 1, except that the ink for forming the primer layer was changed to that used in Example 1.

【0024】単層仕様における性能比較 単層仕様の実施例1、比較例2及び比較例3の耐候性試
験の測定結果を表1に示す。表1の如く、実施例1では
ウェザオメータ1000時間でも耐候性に問題ないが、
プライマー層、印刷絵柄層及び着色隠蔽層に塩素含有樹
脂を用いた比較例1は、500時間でも印刷絵柄層や着
色隠蔽層の密着性が低下し、これら層の脱落が発生す
る。また、プライマー層のみ塩素非含有の樹脂とした比
較例2では比較例1よりは耐候性が向上するが、500
時間で化粧シートの表面にクラックが発生してしまう。
Performance Comparison in Single-Layer Specification Table 1 shows the measurement results of the weather resistance test of Examples 1, 2 and 3 of the single-layer specification. As shown in Table 1, in Example 1, the weather resistance did not have any problem even when the weatherometer was used for 1000 hours.
In Comparative Example 1 in which a chlorine-containing resin was used for the primer layer, the printed pattern layer, and the colored concealing layer, the adhesion of the printed pattern layer and the colored concealing layer was reduced even after 500 hours, and these layers dropped off. Further, in Comparative Example 2 in which only the primer layer contained no chlorine-containing resin, the weather resistance was improved as compared with Comparative Example 1, but 500%.
Cracks occur on the surface of the decorative sheet over time.

【0025】[0025]

【表1】 △:表面クラック発生 ×:印刷絵柄層等の脱落[Table 1] △: Surface crack generation ×: Dropout of printed picture layer etc.

【0026】《実施例2》着色隠蔽オレフィン系樹脂層
として、厚み10μmのポリエチレン製シート、(タノ
ツ化学(株)製、タフパー)を用い、これに、実施例1
と同一インクでプライマー層、印刷絵柄層を形成し、ベ
ースシートとした。一方、透明オレフィン系樹脂層用と
しては、実施例1と同一のポリオレフィン系熱可塑性エ
ラストマーシートにコロナ処理したものを用い、このコ
ロナ処理面にポリエステル系2液硬化型インク(昭和イ
ンク工業(株)製、SPPプライマー)にてプライマー
層をグラビア印刷で形成してトップシートとした。次い
で、前記ベースシートと上記トップシートとを、ダブリ
ングエンボス機により、熱ラミネートすると同時にトッ
プシート表面に熱エンボス加工をして、エンボスによる
凹凸模様表面に有する、本発明の化粧シートを得た。
Example 2 As a colored concealed olefin-based resin layer, a 10 μm-thick polyethylene sheet (Toughper, manufactured by Tanoto Chemical Co., Ltd.) was used.
A primer layer and a printed picture layer were formed with the same ink as in Example 1 to obtain a base sheet. On the other hand, for the transparent olefin-based resin layer, the same polyolefin-based thermoplastic elastomer sheet as in Example 1 was used, which had been subjected to corona treatment, and the corona-treated surface was treated with a polyester two-component curable ink (Showa Ink Kogyo Co., Ltd.) A primer layer was formed by gravure printing using SPP primer (manufactured by Sapphire Co., Ltd.). Next, the base sheet and the top sheet were thermally laminated by a doubling embossing machine and simultaneously the surface of the top sheet was subjected to hot embossing, thereby obtaining a decorative sheet of the present invention having an embossed pattern surface.

【0027】《実施例3》実施例2において、着色隠蔽
オレフィン系樹脂層として用いるベースシートに施すプ
ライマー層の樹脂を、アクリル系2液硬化型樹脂(昭和
インク工業(株)製、SPAプライマー)に代えた他
は、実施例2と同様にして本発明の化粧シートを得た。
Example 3 In Example 2, the resin of the primer layer applied to the base sheet used as the colored concealed olefin resin layer was an acrylic two-component curable resin (SPA primer, manufactured by Showa Ink Industries, Ltd.) The decorative sheet of the present invention was obtained in the same manner as in Example 2 except for changing the above.

【0028】《比較例3》実施例2において、着色隠蔽
オレフィン系樹脂層として用いるベースシートに施すプ
ライマー層形成用インクを、塩化ビニル−酢酸ビニル共
重合体によるインク(大日本インキ化学工業(株)製、
ディックシール A−100Z)に代え、一方、透明オ
レフィン系樹脂層として用いるトップシートに施すプラ
イマー層形成用インクも上記ベースシート用のものと同
一のものに代え、且つ印刷絵柄層形成用インクも、塩化
ビニル−酢酸ビニル共重合体とアクリル樹脂とを用い
た、柄インク(昭和インク工業(株)製、化Xに代え
た他は、実施例2と同様にして化粧シートを得た。
Comparative Example 3 In Example 2, the primer layer forming ink applied to the base sheet used as the colored concealed olefin-based resin layer was a vinyl chloride-vinyl acetate copolymer ink (Dainippon Ink Chemical Industry Co., Ltd.) ),
Instead of Dick Seal A-100Z), on the other hand, the primer layer forming ink applied to the top sheet used as the transparent olefin-based resin layer is also replaced with the same one for the base sheet, and the printing pattern layer forming ink is also used. A decorative sheet was obtained in the same manner as in Example 2 except that a pattern ink (manufactured by Showa Ink Industry Co., Ltd., Chemical X ) using a vinyl chloride-vinyl acetate copolymer and an acrylic resin was used.

【0029】《比較例4》実施例2において、透明オレ
フィン系樹脂層として用いるトップシートに施すプライ
マー層形成用インクを比較例3で用いた、塩化ビニル−
酢酸ビニル共重合体によるインクに代えた他は、実施例
2と同様にして化粧シートを得た。
Comparative Example 4 The same procedure as in Example 2 was repeated except that the ink for forming a primer layer applied to the top sheet used as the transparent olefin resin layer was used in Comparative Example 3.
A decorative sheet was obtained in the same manner as in Example 2, except that the ink was changed to a vinyl acetate copolymer ink.

【0030】《比較例5》比較例3において、透明オレ
フィン系樹脂層として用いるトップシートに施すプライ
マー層形成用インクを実施例2で用いたポリエステル系
2液硬化型インクに代えた他は、比較例3と同様にして
化粧シートを得た。
Comparative Example 5 Comparative Example 3 was the same as Comparative Example 3, except that the ink for forming a primer layer applied to the top sheet used as the transparent olefin-based resin layer was replaced by the polyester-based two-part curable ink used in Example 2. A decorative sheet was obtained in the same manner as in Example 3.

【0031】2層仕様における性能比較 2層仕様の実施例2、実施例3、及び比較例3〜5の耐
候性試験の測定結果を表2に示す。表2の如く、実施例
2及び3ではウェザオメータ1000時間でも耐候性に
問題はないが、プライマー層、印刷絵柄層に塩素含有樹
脂を用いた比較例3は、500時間でもトップシートと
ベースシートとの密着力が低下し、相互に剥がれてしま
う現象(デラミネーション)が発生する。また、この現
象は、印刷絵柄層及びベースシートのプライマー層に塩
素非含有の樹脂を用いたとしてもトップシートのプライ
マー層に塩素含有樹脂を用いれば、比較例4の如く同様
である。また、印刷絵柄層及びベースシートのプライマ
ー層にたとえ塩素含有樹脂を用いてもトップシートのプ
ライマー層に塩素非含有の樹脂を用いれば、比較例5の
如く化粧シート表面のクラック発生程度まで耐候性はあ
る程度は向上するが、印刷絵柄層及びベースシートのプ
ライマー層に塩素非含有の樹脂を用いる実施例2及び実
施例3に比べれば劣る。
Performance Comparison in Two-Layer Specifications Table 2 shows the measurement results of the weather resistance tests of Examples 2, Example 3, and Comparative Examples 3 to 5 of the two-layer specifications. As shown in Table 2, in Examples 2 and 3, there is no problem in weather resistance even with a weatherometer of 1000 hours, but Comparative Example 3 in which a chlorine-containing resin is used for a primer layer and a printed picture layer has a top sheet and a base sheet that are 500 hours. , A phenomenon (delamination) occurs in which the adhesive strengths of the substrates are separated from each other. This phenomenon is the same as in Comparative Example 4 even if a chlorine-free resin is used for the printed pattern layer and the primer layer of the base sheet, but the chlorine-containing resin is used for the primer layer of the top sheet. Further, even if a chlorine-containing resin is used for the printed pattern layer and the primer layer of the base sheet, if a chlorine-free resin is used for the primer layer of the top sheet, the weather resistance up to the degree of crack generation on the decorative sheet surface as in Comparative Example 5 Is improved to some extent, but is inferior to Examples 2 and 3 in which a chlorine-free resin is used for the printed picture layer and the primer layer of the base sheet.

【0032】[0032]

【表2】 △:表面クラック発生 ×:デラミネーション[Table 2] Δ: Surface crack generation ×: Delamination

【0033】[0033]

【発明の効果】本発明によれば、塩化ビニル樹脂製の化
粧シートの代替材料として、オレフィン系樹脂製の化粧
シートの耐候性について、従来の塩化ビニル樹脂製化粧
シート並の性能が得られる。
According to the present invention, the performance of a decorative sheet made of an olefin-based resin as a substitute for a decorative sheet made of a vinyl chloride resin is as good as that of a conventional decorative sheet made of a vinyl chloride resin.

【図面の簡単な説明】[Brief description of the drawings]

【図1】本発明の化粧シートの一形態を示す断面図(単
層仕様)。
FIG. 1 is a cross-sectional view (single-layer specification) showing one embodiment of a decorative sheet of the present invention.

【図2】本発明の化粧シートの他の形態を示す断面図
(2層仕様)。
FIG. 2 is a cross-sectional view (two-layer specification) showing another embodiment of the decorative sheet of the present invention.

【図3】本発明の化粧シートの他の形態を示す断面図。FIG. 3 is a sectional view showing another embodiment of the decorative sheet of the present invention.

【図4】本発明の化粧シートの他の形態を示す断面図。FIG. 4 is a sectional view showing another embodiment of the decorative sheet of the present invention.

【符号の説明】[Explanation of symbols]

1 透明オレフィン系樹脂層 2 印刷絵柄層 3 着色隠蔽層 4 着色オレフィン系樹脂層 5 プライマー層 10 化粧シート(単層仕様) 20 化粧シート(2層仕様) DESCRIPTION OF SYMBOLS 1 Transparent olefin resin layer 2 Print pattern layer 3 Color hiding layer 4 Color olefin resin layer 5 Primer layer 10 Decorative sheet (single-layer specification) 20 Decorative sheet (2-layer specification)

───────────────────────────────────────────────────── フロントページの続き (51)Int.Cl.7 識別記号 FI C08L 23/00 C08L 23/00 E04F 13/00 E04F 13/00 B 13/18 13/18 A (56)参考文献 特開 平8−34058(JP,A) 特開 平8−90740(JP,A) 特開 平6−198831(JP,A) 特開 平8−34105(JP,A) (58)調査した分野(Int.Cl.7,DB名) B32B 33/00 B32B 27/32 B32B 31/00 E04F 13/00 E04F 13/18 ────────────────────────────────────────────────── ─── Continuation of the front page (51) Int.Cl. 7 Identification code FI C08L 23/00 C08L 23/00 E04F 13/00 E04F 13/00 B 13/18 13/18 A (56) References 8-34058 (JP, A) JP-A-8-90740 (JP, A) JP-A-6-198831 (JP, A) JP-A-8-34105 (JP, A) (58) Fields investigated (Int. Cl. 7 , DB name) B32B 33/00 B32B 27/32 B32B 31/00 E04F 13/00 E04F 13/18

Claims (2)

(57)【特許請求の範囲】(57) [Claims] 【請求項1】 表側より順に透明オレフィン系樹脂層、
印刷絵柄層、着色隠蔽層からなると共に、該着色隠蔽層
を被着体適用表面とする化粧シートにおいて、透明オレ
フィン系樹脂層がヒンダードアミン系光安定剤を含有
し、且つ印刷絵柄層及び着色隠蔽層が塩素を含まない
硬化性樹脂からなる、耐候性のあるオレフィン系化粧シ
ート。
1. A transparent olefin resin layer in order from the front side,
Printing pattern layer, Rutotomoni such a colored concealing layer, colored concealing layer
The in decorative sheet to an adherend application surface, a transparent olefin resin layer contains a hindered amine light stabilizer, and print pattern layer and the colored concealing layer does not contain chlorine heat
A weather-resistant olefin-based decorative sheet made of a curable resin.
【請求項2】 表側より順に透明オレフィン系樹脂層、
プライマー層、印刷絵柄層、プライマー層、着色オレフ
ィン系樹脂層よりなる化粧シートにおいて、透明オレフ
ィン系樹脂層がヒンダードアミン系光安定剤を含有し、
且つプライマー層及び印刷絵柄層が塩素を含まない熱硬
化性樹脂からなる、耐候性のあるオレフィン系化粧シー
ト。
2. A transparent olefin resin layer in order from the front side,
In a decorative sheet comprising a primer layer, a printed picture layer, a primer layer and a colored olefin resin layer, the transparent olefin resin layer contains a hindered amine light stabilizer,
Heat-hardened primer layer and printed picture layer do not contain chlorine
A weather-resistant olefin-based decorative sheet made of a curable resin.
JP15287896A 1996-05-27 1996-05-27 Olefin-based decorative sheet with weather resistance Expired - Fee Related JP3156150B2 (en)