WO2025044002A1 - 一种太阳能电池组件的制备方法 - Google Patents
一种太阳能电池组件的制备方法 Download PDFInfo
- Publication number
- WO2025044002A1 WO2025044002A1 PCT/CN2023/142198 CN2023142198W WO2025044002A1 WO 2025044002 A1 WO2025044002 A1 WO 2025044002A1 CN 2023142198 W CN2023142198 W CN 2023142198W WO 2025044002 A1 WO2025044002 A1 WO 2025044002A1
- Authority
- WO
- WIPO (PCT)
- Prior art keywords
- light
- adhesive film
- transmitting adhesive
- liquid
- solar cell
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Ceased
Abstract
本申请提供一种太阳能电池组件的制备方法,包括:提供第一封装层;在第一封装层的一侧形成阻水胶层;在第一封装层的一侧的电池组放置区形成液态或半液半固态的第一透光胶膜;在第一透光胶膜背离第一封装层的一侧表面铺设太阳能电池组;在太阳能电池组背离第一透光胶膜的一侧表面形成液态或半液半固态的第二透光胶膜;在阻水胶层和第二透光胶膜背离第一封装层的一侧设置第二封装层;对包括第一封装层、第一透光胶膜、太阳能电池组、第二透光胶膜和第二封装层的结构进行层压,层压后使得第一透光胶膜和第二透光胶膜熔融后固化,第一透光胶膜和第二透光胶膜均与阻水胶层接触。该制备方法形成的太阳能电池组件光电转换效率、功率和可靠性得到提高。
Description
相关申请的交叉引用
本申请要求在2023年8月31日提交中国专利局、申请号为202311124825.X、发明名称为“一种太阳能电池组件的制备方法”的中国专利申请的优先权,其全部内容通过引用的方式并入本文中。
本申请涉及太阳能电池制造技术领域,具体涉及一种太阳能电池组件的制备方法。
异质结电池技术作为近年来引起行业高度关注的高效技术路线,因其功率高、光电转换效率高、性能优异、降本空间大,成为行业公认的未来电池技术终极解决方案,并一度被业内称为是下一代商业光伏生产的前沿技术,但高效率异质结太阳能电池组在经过封装形成太阳能电池组件后效率不能得到充分利用。一方面原因,因玻璃透光率最高在94.3%附近,封装胶膜透光率在90%附近;另一方面,异质结太阳能电池的透明导电层(TCO层)使用的ITO材料对水汽十分敏感,遇水汽会出现比较明显的电性能损失,造成太阳能电池组件的功率下降,此外,太阳能电池组件在运输过程中容易受到机械碰撞,以及在平放过程中受到自然重力会发生抖动,会导致太阳能电池组件中的太阳能电池片发生裂片的风险。
因此,需要提供一种具有更高光电转换效率和可靠性的太阳能电池组件,相应的需要对制备方法进行改进。
发明内容
因此,本申请要解决的技术问题在于克服现有太阳能电池组件的制备方法形成的太阳能电池组件的光电转换效率和可靠性较低的缺陷,进而提供一种太阳能电池组件的制备方法。
本申请提供一种太阳能电池组件的制备方法,包括:提供第一封装层,所述第一封装层包括电池组放置区和环绕所述电池组放置区的边缘区;在所述第一封装层的一侧的边缘区形成阻水胶层;在所述第一封装层的一侧的电池组放置区形成液态或半液半固态的第一透光胶膜,所述第一透光胶膜与所述阻水胶层位于所
述第一封装层的同侧;在所述第一透光胶膜背离所述第一封装层的一侧表面铺设太阳能电池组;在所述太阳能电池组背离所述第一透光胶膜的一侧表面形成液态或半液半固态的第二透光胶膜;在所述阻水胶层和所述第二透光胶膜背离所述第一封装层的一侧设置第二封装层,所述阻水胶层的厚度等于或者大于所述第二透光胶膜背离所述第一封装层一侧表面至所述第一封装层的距离;对包括所述第一封装层、所述第一透光胶膜、所述太阳能电池组、所述第二透光胶膜和所述第二封装层的结构进行层压,层压后使得所述第一透光胶膜和所述第二透光胶膜熔融后固化,所述第一透光胶膜和所述第二透光胶膜均与所述阻水胶层接触。
可选的,在所述第一封装层的一侧的电池组放置区形成液态或半液半固态的第一透光胶膜的步骤中,所述第一透光胶膜和所述阻水胶层之间具有间隙;对所述第一封装层、所述第一透光胶膜、所述太阳能电池组、所述第二透光胶膜和所述第二封装层进行层压的步骤中,所述第一透光胶膜和/或第二透光胶膜填充所述间隙。
可选的,所述间隙的宽度尺寸为2mm~8mm。
可选的,所述阻水胶层的厚度比所述第二透光胶膜背离所述第一封装层一侧表面至所述第一封装层的距离大0.2mm~0.5mm。
可选的,液态或半液半固态的第一透光胶膜的粘稠度为40000mpa.s~60000mpa.s;液态或半液半固态的第二透光胶膜的粘稠度为40000mpa.s~60000mpa.s。
可选的,形成液态或半液半固态的第一透光胶膜采用的工艺包括喷涂工艺或丝网印刷工艺;形成液态或半液半固态第二透光胶膜采用的工艺包括喷涂工艺或丝网印刷工艺。
可选的,形成液态或半液半固态的第一透光胶膜采用的工艺包括喷涂工艺;形成液态或半液半固态的第一透光胶膜的步骤中:沿着第一方向和第二方向交错进行喷涂;所述第一方向与第二方向垂直;形成液态或半液半固态的第二透光胶膜采用的工艺包括喷涂工艺;形成液态或半液半固态的第二透光胶膜的步骤中:沿着第一方向和第二方向交错进行喷涂;所述第一方向与第二方向垂直。
可选的,对所述第一封装层、所述第一透光胶膜、所述太阳能电池组、所述第二透光胶膜和所述第二封装层进行层压的参数包括:层压的温度为:70℃~120℃;层压的时间为:660s~700s,层压的压强为35kPa~75kPa。
可选的,对所述第一封装层、所述第一透光胶膜、所述太阳能电池组、所述第二透光胶膜和所述第二封装层进行层压的过程包括:依次进行的第一次层压、第二次层压和第三次层压,第一次层压、第二次层压和第三次层压的压强递减。
可选的,第一次层压的压强为65kPa~75kPa;第二次层压的压强为45kPa~55kPa;第三次层压的压强为35kPa~45kPa。
可选的,第一次层压的时间为15s~25s;第二次层压的时间为15s~25s;第三次层压的时间为630s~650s。
可选的,在所述第一封装层的一侧的电池组放置区形成液态或半液半固态的第一透光胶膜的步骤中,所述第一透光胶膜的厚度为0.3mm~0.8mm;在所述太阳能电池组背离所述第一透光胶膜的一侧表面形成液态或半液半固态的第二透光胶膜的步骤中,所述第二透光胶膜的厚度为0.3mm~0.8mm。
可选的,所述第一透光胶膜的材料包括液态硅胶、硅胶、液态硅橡胶、液态胶、凝胶、有机硅凝胶、硅体胶、硅橡胶、液态原料、硅橡胶胶料和硅橡胶原料中的至少一种;所述第二透光胶膜的材料包括液态硅胶、硅胶、液态硅橡胶、液态胶、凝胶、有机硅凝胶、硅体胶、硅橡胶、液态原料、硅橡胶胶料和硅橡胶原料中的至少一种。
可选的,对所述第一封装层、所述第一透光胶膜、所述太阳能电池组、所述第二透光胶膜和所述第二封装层进行层压之前,所述阻水胶层的宽度为2mm~15mm,所述阻水胶层的厚度为0.5mm~3.5mm。
可选的,所述阻水胶层的材料包括异丁烯类聚合物、异戊二烯类聚合物中的任意一种。
本申请技术方案,具有如下优点:
本申请提供的太阳能电池组件的制备方法,在所述第一封装层的一侧的边缘区形成阻水胶层;在所述第一封装层的一侧的电池组放置区形成液态或半液半固态的第一透光胶膜,所述第一透光胶膜与所述阻水胶层位于所述第一封装层的同侧;在所述第一透光胶膜背离所述第一封装层的一侧表面铺设太阳能电池组;在所述太阳能电池组背离所述第一透光胶膜的一侧表面形成液态或半液半固态的第二透光胶膜;在所述阻水胶层和所述第二透光胶膜背离所述第一封装层的一侧设置第二封装层,所述阻水胶层的厚度等于或者大于所述第二透光胶膜背离所述第一封装层一侧表面至所述第一封装层的距离;对包括所述第一封装层、第一透光胶膜、太阳能电池组、第二透光胶膜和第二封装层进行层压,层压后使得所述第一透光胶膜和所述第二透光胶膜熔融后固化,所述第一透光胶膜和所述第二透光胶膜均与所述阻水胶层接触。首先,所述第一透光胶膜和所述第二透光胶膜具有高透光率且无黄变的特性,因此,可以提高太阳能电池组件的透光率、光电转换效率和功率;其次,所述第一透光胶膜和所述第二透光胶膜具有耐老化的特性,且所述第一透光胶膜、所述第二透光胶膜和所述阻水胶层形成了一个封闭绝缘的
空间,可以高效地阻挡外界水汽、粉尘等浸入太阳能电池组件的内部,提高了太阳能电池组件的阻水汽性能和耐气候性能;再次,所述第一透光胶膜和所述第二透光胶膜具有柔软性的特性,在太阳能电池组件受到机械碰撞时,所述第一透光胶膜和所述第二透光胶膜可以对太阳能电池组起到缓冲保护的作用,因此,所述太阳能电池组件的可靠性高。综上,所述太阳能电池组件的制备方法形成的太阳能电池组件的光电转换效率、功率和可靠性高。
为了更清楚地说明本申请具体实施方式或现有技术中的技术方案,下面将对具体实施方式或现有技术描述中所需要使用的附图作简单地介绍,显而易见地,下面描述中的附图是本申请的一些实施方式,对于本领域普通技术人员来讲,在不付出创造性劳动的前提下,还可以根据这些附图获得其他的附图。
图1为本申请一实施例提供的太阳能电池组件制备方法的流程图;
图2至图9为本申请一实施例提供的太阳能电池组件制备过程的结构示意图;
图10为采用本实施例提供的太阳能电池组件的制备方法形成的太阳能电池组件与采用常规高透胶膜封装形成的太阳能电池组件的光谱响应程度对比图。
附图标记说明:
1-第一封装层;11-电池组放置区;12-边缘区;13-阻水胶层;
21-第一透光胶膜;
3-太阳能电池组;
22-第二透光胶膜;
4-第二封装层;
L-间隙;X-第一方向;Y-第二方向。
1-第一封装层;11-电池组放置区;12-边缘区;13-阻水胶层;
21-第一透光胶膜;
3-太阳能电池组;
22-第二透光胶膜;
4-第二封装层;
L-间隙;X-第一方向;Y-第二方向。
下面将结合附图对本申请的技术方案进行清楚、完整地描述,显然,所描述的实施例是本申请一部分实施例,而不是全部的实施例。基于本申请中的实施例,本领域普通技术人员在没有做出创造性劳动前提下所获得的所有其他实施例,都属于本发明保护的范围。
在本申请的描述中,需要说明的是,术语“中心”、“上”、“下”、“左”、“右”、“竖直”、“水平”、“内”、“外”等指示的方位或位置关系为基于附图所示的方位或位置关系,仅是为了便于描述本申请和简化描述,而不是指示
或暗示所指的装置或元件必须具有特定的方位、以特定的方位构造和操作,因此不能理解为对本申请的限制。此外,术语“第一”、“第二”、“第三”仅用于描述目的,而不能理解为指示或暗示相对重要性。
在本申请的描述中,需要说明的是,除非另有明确的规定和限定,术语“安装”、“相连”、“连接”应做广义理解,例如,可以是固定连接,也可以是可拆卸连接,或一体地连接;可以是机械连接,也可以是电连接;可以是直接相连,也可以通过中间媒介间接相连,可以是两个元件内部的连通。对于本领域的普通技术人员而言,可以具体情况理解上述术语在本申请中的具体含义。
此外,下面所描述的本申请不同实施方式中所涉及的技术特征只要彼此之间未构成冲突就可以相互结合。
本实施例提供一种太阳能电池组件的制备方法,参考图1,包括以下步骤:
步骤S1:提供第一封装层,所述第一封装层包括电池组放置区和环绕所述电池组放置区的边缘区;
步骤S2:在所述第一封装层的一侧的边缘区形成阻水胶层;
步骤S3:在所述第一封装层的一侧的电池组放置区形成液态或半液半固态的第一透光胶膜,所述第一透光胶膜与所述阻水胶层位于所述第一封装层的同侧;
步骤S4:在所述第一透光胶膜背离所述第一封装层的一侧表面铺设太阳能电池组;
步骤S5:在所述太阳能电池组背离所述第一透光胶膜的一侧表面形成液态或半液半固态的第二透光胶膜;
步骤S6:在所述阻水胶层和所述第二透光胶膜背离所述第一封装层的一侧设置第二封装层,所述阻水胶层的厚度等于或者大于所述第二透光胶膜背离所述第一封装层一侧表面至所述第一封装层的距离;
步骤S7:对包括所述第一封装层、第一透光胶膜、太阳能电池组、第二透光胶膜和第二封装层的结构进行层压,层压后使得所述第一透光胶膜和所述第二透光胶膜熔融后固化,所述第一透光胶膜和所述第二透光胶膜均与所述阻水胶层接触。
本实施例提供的太阳能电池组件的制备方法,所述第一透光胶膜和所述第二透光胶膜均与所述阻水胶层接触,首先,所述第一透光胶膜和所述第二透光胶膜具有高透光率且无黄变的特性,因此,可以提高太阳能电池组件的透光率、光电转换效率和功率,其次,所述第一透光胶膜和所述第二透光胶膜具有耐老化的特性,且所述第一透光胶膜、所述第二透光胶膜和所述阻水胶层形成了一个封闭绝
缘的空间,可以高效地阻挡外界水汽、粉尘等浸入太阳能电池组件的内部,提高了太阳能电池组件的阻水汽性能和耐气候性能;再次,所述第一透光胶膜和所述第二透光胶膜具有柔软性的特性,在太阳能电池组件受到机械碰撞时,所述第一透光胶膜和所述第二透光胶膜可以对太阳能电池组起到缓冲保护的作用,因此,所述太阳能电池组件的可靠性高。综上,所述太阳能电池组件的制备方法形成的太阳能电池组件的光电转换效率、功率和可靠性高。
对所述第一封装层、第一透光胶膜、太阳能电池组、第二透光胶膜和第二封装层进行层压的步骤中,所述第一透光胶膜的和/或第二透光胶膜填充所述间隙。该空隙被具有高透光率且无黄变的特性的第一透光胶膜和所述第二透光胶膜填充,在太阳能电池组充分利用光照的同时,侧部的第一透光胶膜和第二透光胶膜可以提高对来自侧部的光照的利用率,进而增加太阳能电池组件的光电转化效率。
下面参考图2至图9详细介绍所述太阳能电池组件的制备方法。
参考图2,提供第一封装层1,所述第一封装层1包括电池组放置区11和环绕所述电池组放置区11的边缘区12。
在一个实施例中,所述第一封装层1包括玻璃,玻璃为光伏行业通用的光伏玻璃。
参考图3,在所述第一封装层1的一侧的边缘区12形成阻水胶层13。
在一个实施例中,形成阻水胶层13的方式包括桶装胶打胶的方式或者直接敷设胶带的方式。
在一个实施例中,阻水胶层13包括透明阻水胶层和非透明阻水胶层。
在一个实施例中,所述阻水胶层13的宽度为2mm~15mm,例如3mm、5mm、8mm、10mm、12mm或者14mm;若所述阻水胶层13的宽度小于2mm,若所述阻水胶层的宽度小于2mm,则所述阻水胶层起到阻止环境中的水汽与粉尘穿过所述阻水胶层渗入到所述太阳能电池组的作用较弱;若所述阻水胶层13的宽度大于15mm,则阻水胶层的宽度过大,则在层压时可能导致所述阻水胶层溢出,造成浪费。
在一个实施例中,所述阻水胶层13的厚度为0.5mm~3.5mm,例如1mm、1.5mm、2mm、2.5mm或者3mm;若所述阻水胶层13的厚度小于0.5mm,则阻水胶层的厚度过小可能使太阳能电池组处于完全封闭的环境的程度较小,起到阻挡水汽的作用较小;若所述阻水胶层13的厚度大于3.5mm,则在层压过程中容易溢胶,造成资源浪费。
在一个实施例中,所述阻水胶层13的材料包括异丁烯类聚合物、异戊二烯类
聚合物中的任意一种;在其他实施例中,所述阻水胶层的材料还可以包括其他具备高性能阻水汽能力以及防老化能力的其他丁基胶材料。
参考图4,在所述第一封装层1的一侧的电池组放置区11形成液态或半液半固态的第一透光胶膜21,所述第一透光胶膜21与所述阻水胶层13位于所述第一封装层1的同侧。
在一个实施例中,所述第一透光胶膜21的材料包括液态硅胶、硅胶、液态硅橡胶、液态胶、凝胶、有机硅凝胶、硅体胶、硅橡胶、液态原料、硅橡胶胶料和硅橡胶原料中的至少一种。
在一个实施例中,继续参考图4,在所述第一封装层1的一侧的电池组放置区11形成液态或半液半固态的第一透光胶膜的步骤中,所述第一透光胶膜21和所述阻水胶层13之间具有间隙L。
在一个实施例中,所述间隙L的尺寸为2mm~8mm,例如2.5mm、3mm、3.5mm、4mm、4.5mm、5.5mm或者6.5mm;若所述第一透光胶膜21和所述阻水胶层13之间的间隙L小于2mm,则在层压过程中,所述阻水胶层可能溢到所述第一透光胶膜上;若所述第一透光胶膜21和所述阻水胶层13之间的间隙L大于8mm,则最终形成的太阳能电池组件中,所述阻水胶层与所述第一透光胶膜以及阻水胶层与所述第二透光胶膜之间可能会仍然存在空隙导致容易形成气泡,影响太阳能电池组件的外观和耐候性能。为了避免在层压后阻水胶层与第一透光胶膜之间以及阻水胶层与第二透光胶膜之间存在气泡,在所述第一封装层的一侧的电池组放置区形成液态或半液半固态的第一透光胶膜之前,以及在所述太阳能电池组背离所述第一透光胶膜的一侧表面形成液态或半液半固态的第二透光胶膜之前,还包括:对第一透光胶膜的材料和第二透光胶膜的材料进行去除气泡处理,去除气泡处理的方式包括对第一透光胶膜的材料和第二透光胶膜的材料采用抽真空与烘烤结合、离心或者静置处理的方式。其中,静止处理的时间为30分钟~2小时,静止处理可以使得第一透光胶膜的材料和第二透光胶膜的材料中的气泡自己浮到表面并排出;离心的方式为:按顺时针方向对第一透光胶膜的材料和第二透光胶膜的材料搅拌2分钟~3分钟,搅拌均匀后将第一透光胶膜的材料和第二透光胶膜的材料放置520分钟自动脱泡,该种方法只针对于粘度较稀的第一透光胶膜的材料和第二透光胶膜的材料,如果第一透光胶膜的材料和第二透光胶膜的材料很稠,滞留其中的气泡不易升起排出。另外,采用抽真空与烘烤结合的方法,还有利于让第一透光胶膜的材料和第二透光胶膜的材料中的杂质挥发。
在一个实施例中,在所述第一封装层1的一侧的电池组放置区11形成液态或半液半固态的第一透光胶膜21的步骤中,所述第一透光胶膜21的厚度为
0.3mm~0.8mm,例如0.35mm、0.4mm、0.45mm、0.5mm、0.55mm、0.6mm或者0.65mm;若所述第一透光胶膜21的厚度小于0.3mm,则在太阳能电池组件受到机械碰撞时,所述第一透光胶膜对太阳能电池组起到缓冲保护的效果不明显;若所述第一透光胶膜21的厚度大于0.8mm,则在层压过程中第一透光胶膜容易溢出,造成资源浪费。
在一个实施例中,形成液态或半液半固态的第一透光胶膜采用的工艺包括喷涂工艺或丝网印刷工艺,喷涂工艺包括桶装打胶方式或点胶方式。
在一个实施例中,液态或半液半固态的第一透光胶膜的粘稠度为40000mpa.s~60000mpa.s,例如45000mpa.s、50000mpa.s或者55000mpa.s,若液态或半液半固态的第一透光胶膜的粘稠度小于40000mpa.s,则第一透光胶膜的粘稠度太低,会造成固化时间过长;若液态或半液半固态的第一透光胶膜的粘稠度大于60000mpa.s,则第一透光胶膜的粘稠度太高使得流动性差,固化的时间太短,自动填充电池片之间间隙的效果不明显。因此第一透光胶膜的粘稠度选择40000mpa.s~60000mpa.s,能兼顾固化时间短和填充太阳能电池组中相邻电池片之间间隙的效果较好。
在一个实施例中,结合参考图4和图5,形成液态或半液半固态的第一透光胶膜采用的工艺包括喷涂工艺;形成液态或半液半固态的第一透光胶膜的步骤中:沿着第一方向X和第二方向Y交错进行喷涂;所述第一方向X与第二方向Y垂直;所述第一方向X与所述第一封装层的侧边平行。
参考图6,在所述第一透光胶膜21背离所述第一封装层1的一侧表面铺设太阳能电池组3。在所述第一透光胶膜21背离所述第一封装层1的一侧表面铺设太阳能电池组3的过程中,所述第一封装层和所述第一透光胶膜保持水平放置,采用吸盘将太阳能电池组吸附,精确定位后,放置在所述第一透光胶膜21背离所述第一封装层1的一侧表面,位于电池组放置区11内。
在一个实施例中,太阳能电池组3的形成步骤包括:通过串焊机将用激光切割好的太阳能电池片依次排列,所述太阳能电池片包括半片电池片,之后通过互联条对太阳能电池片依次串联进行焊接;焊接后,形成串联的若干串太阳能电池串;之后,通过排版机将串联好的若干串太阳能电池串按照电极顺序依次排列,完成多串太阳能电池串的铺设,然后通过叠焊机用汇流条将太阳能电池串并联连接起来,并留出引线以便于与后面工序的接线盒安装,汇流焊接完成后形成太阳能电池串方阵;再通过胶带对太阳能电池串方阵进行定位,将太阳能电池串方阵进行定位形成太阳能电池组。
在一个实施例中,所述太阳能电池片包括无主栅线印刷的双面异质结太阳电
池片,所述太阳能电池片表面设置有透明导电膜(TCO),透明导电膜为ITO膜或AZO膜;汇流条为光伏行业通用焊带。
在一个实施例中,在所述第一透光胶膜21背离所述第一封装层1的一侧表面铺设太阳能电池组3之后还包括:对所述太阳能电池组3进行缺陷检测,对有缺陷的太阳能电池组进行返修,这样操作与在形成太阳能电池组件后再进行缺陷检测相比,有利于避免造成大量的重复返工工作量,有利于减少人工成本,有利于提高生产线利用率和生产效率,也有利于降低返修成本。
对所述太阳能电池组进行缺陷检测包括:外观形貌检测、隐裂检测和虚焊检测中的一种或者几种,外观形貌检测为检测所述太阳能电池组是否存在破损,隐裂检测为检测所述太阳能电池组中的太阳能电池是否存在裂片,虚焊检测为检测所述太阳能电池组中的太阳能电池与焊带之间是否存在虚焊。
在一个实施例中,对所述太阳能电池组进行所述隐裂检测时,检测到所述太阳能电池组中的太阳能电池存在裂片,则需对存在裂片的太阳能电池组进行返修,直至对所述太阳能电池组检验合格。
在另一个实施例中,对所述太阳能电池组进行所述虚焊检测时,检测到所述太阳能电池组中的太阳能电池与焊带之间存在虚焊,则需对存在虚焊的太阳能电池与焊带之间存在虚焊位置重新焊接,直至对所述太阳能电池组检验合格。
参考图7,在所述太阳能电池组3背离所述第一透光胶膜21的一侧表面形成液态或半液半固态的第二透光胶膜22。
在一个实施例中,所述第二透光胶膜22的材料包括液态硅胶、硅胶、液态硅橡胶、液态胶、凝胶、有机硅凝胶、硅体胶、硅橡胶、液态原料、硅橡胶胶料和硅橡胶原料中的至少一种。
在一个实施例中,在所述太阳能电池组3背离所述第一透光胶膜21的一侧表面形成液态或半液半固态的第二透光胶膜22的步骤中,所述第二透光胶膜22的厚度为0.3mm~0.8mm,例如0.35mm、0.4mm、0.45mm、0.5mm、0.55mm、0.6mm或者0.65mm;若所述第二透光胶膜22的厚度小于0.3mm,则在太阳能电池组件受到机械碰撞时,所述第二透光胶膜对太阳能电池组起到缓冲保护的效果不明显;若所述第二透光胶膜22的厚度大于0.8mm,则在层压过程中第二透光胶膜容易溢出,造成资源浪费。
在一个实施例中,所述阻水胶层的厚度比所述第二透光胶膜背离所述第一封装层一侧表面至所述第一封装层的距离大0.2mm~0.5mm,例如0.3mm,这样有利于所述第一透光胶膜、所述第二透光胶膜和所述阻水胶层形成一个封闭绝缘的空间,可以高效地阻挡外界水汽、粉尘等浸入太阳能电池组件的内部,提高了太阳能电池组件的阻水汽性能和耐气候性能。
在一个实施例中,形成液态或半液半固态的第二透光胶膜22采用的工艺包括喷涂工艺或丝网印刷工艺,喷涂工艺包括桶装打胶方式或点胶方式。
在一个实施例中,液态或半液半固态的第二透光胶膜的粘稠度为40000mpa.s~60000mpa.s,例如45000mpa.s、50000mpa.s或者55000mpa.s,若液态或半液半固态的第二透光胶膜的粘稠度小于40000mpa.s,则第二透光胶膜的粘稠度太低,会造成固化时间过长;若液态或半液半固态的第二透光胶膜的粘稠度大于60000mpa.s,则第二透光胶膜的粘稠度太高使得流动性差,固化的时间太短,自动填充电池片之间间隙的效果不明显。本实施例中将第二透光胶膜的粘稠度选择为40000mpa.s~60000mpa.s,能兼顾固化时间短和填充电池片之间间隙的效果较好。
在一个实施例中,形成液态或半液半固态的第二透光胶膜采用的工艺包括喷涂工艺;形成液态或半液半固态的第二透光胶膜的步骤中:沿着第一方向和第二方向交错进行喷涂;所述第一方向与第二方向垂直所述第一方向与所述第一封装层的侧边平行。
参考图8,在所述阻水胶层13和所述第二透光胶膜22背离所述第一封装层1的一侧设置第二封装层4。具体的,采用合玻机或者铺设机在所述阻水胶层13和所述第二透光胶膜22背离所述第一封装层1的一侧设置第二封装层4,所述第一封装层、第一透光胶膜、太阳能电池组、第二透光胶膜和第二封装层构成太阳能电池组件层叠件。
在一个实施例中,所述第二封装层4包括玻璃,玻璃为光伏行业通用的光伏玻璃。
参考图9,图9为对图8中的第一封装层、第一透光胶膜、太阳能电池组、第二透光胶膜和第二封装层进行层压之后的示意图,层压后第一透光胶膜和第二透光胶膜以及阻水胶层对太阳能电池组形成密封包裹,对所述第一封装层、第一透光胶膜、太阳能电池组、第二透光胶膜和第二封装层进行层压,层压的同时使所述第一透光胶膜和所述第二透光胶膜熔融并固化,所述第一透光胶膜和所述第二透光胶膜均与所述阻水胶层接触。
在一个实施例中,在所述阻水胶层13和所述第二透光胶膜22背离所述第一封装层1的一侧设置第二封装层4之后,对所述第一封装层、第一透光胶膜、太阳能电池组、第二透光胶膜和第二封装层进行层压之前,还包括:对太阳能电池组件层叠件进行缺陷检测,如发现问题则将不合格的太阳能电池组件层叠件放置返修台及时返修,将对所述第一封装层、第一透光胶膜、太阳能电池组、第二透光胶膜和第二封装层进行层压之前的缺陷先行排除,完成后才进行层压,并对层
压之后的太阳能电池组件整体进行检测及返修,严保产品质量。这样,减小了在返修时将第一封装层和第二封装层分离的难度,也减小了在分离时用力过大造成所述太阳能电池组发生隐裂与破片几率,因此,所述太阳能电池组件的制备方法的封装效率与良率高。太阳能电池组件需要层压前检测,确保有缺陷产品可以返修。层压后成层压件,无法返修,只能通过检验识别太阳能电池组件确认质量级别。
在一个实施例中,对所述第一封装层、第一透光胶膜、太阳能电池组、第二透光胶膜和第二封装层进行层压之前,还包括:对层压机的腔体进行抽真空处理,所述抽真空处理的时间为280s~320s,例如为290s、300s或310s,若对层压机的腔体进行抽真空处理的时间少于280s,则抽出所述电池组件层叠件中的气体不够彻底,容易导致所述第一透光胶膜与所述太阳能电池组之间、所述第二透光胶膜与所述太阳能电池组之间,所述第一封装层与所述第一透光胶膜之间,所述第二封装层与所述第二透光胶膜之间存在气泡,影响太阳能电池组件的外观和耐候性能。
在一个实施例中,对所述第一封装层1、第一透光胶膜21、太阳能电池组3、第二透光胶膜22和第二封装层4进行层压的参数包括:层压的温度为:70℃~120℃,例如100℃;层压的时间为:660s~700s,例如690s;层压的压强为35kPa~75kPa,例如70kPa。
在一个实施例中,对所述第一封装层1、第一透光胶膜21、太阳能电池组3、第二透光胶膜22和第二封装层4进行层压的过程包括:依次进行的第一次层压、第二次层压和第三次层压,第一次层压、第二次层压和第三次层压的压强递减。第一次层压的时间为15s~25s,例如20s;第一次层压的压强为65kPa~75kPa,例如70kPa;第二次层压的时间为15s~25s,例如20s;第二次层压的压强为45kPa~55kPa,例如50kPa;第三次层压的时间为630s~650s,例如640s;第三次层压的压强为35kPa~45kPa,例如40kPa。将所述第一封装层1、第一透光胶膜21、太阳能电池组3、第二透光胶膜22和第二封装层4进行层压分成三次层压,这样有利于使得所述第一透光胶膜21和所述第二透光胶膜22固化完全。
在一个实施例中,对所述第一封装层1、第一透光胶膜21、太阳能电池组3、第二透光胶膜22和第二封装层4层压之后还包括:对层压之后的电池组件层叠件进行外观检测和修边处理。
在一个实施例中,第一透光胶膜和第二透光胶膜均为A型和B型混合型胶,混合比例1:1,单一A型或B型胶不发生固化,混合后在25摄氏度室温下固化所需时间大于6小时,当层压温度大于70摄氏度时,液态硅胶透光率在94%以上,黄变指数和雾度小于0.2%,体积收缩小于0.1%。
在一个实施例中,所述太阳能电池组件的制备方法,还包括:提供封装框(附图中未示出),所述封装框中具有容纳腔,在所述容纳腔的内壁表面形成边框胶;之后,将层压之后的电池组件的边缘区域套在所述容纳腔中。
在一个实施例中,在所述阻水胶层13和所述第二透光胶膜22背离所述第一封装层1的一侧设置第二封装层4之前,还包括:形成引线孔,引线孔的数量为3个,3个引线孔间隔排布,任意一个引线孔的直径为9mm~13mm,所述第二封装层背离所述第一封装层的一侧表面铺设有离心纸,离心纸覆盖引线孔,离心纸上设置有允许汇流条通过的通道,离心纸为耐高温材料,在高温条件下,例如150摄氏度,离心纸不收缩,不融化。所述引线孔在垂直于第一封装层1的方向上还贯穿所述第二封装层和所述第二透光胶膜,在所述阻水胶层13和所述第二透光胶膜22背离所述第一封装层1的一侧设置第二封装层4的过程中,将所述汇流条穿过所述引线孔;之后,在所述引线孔中形成密封填充胶,之后,对所述密封填充胶进行固化处理。在一个实施例中,所述太阳能电池组件的制备方法还包括功率测试、终检工序。
液态硅胶固化后形成的第一透光胶膜和第二透光胶膜可以将紫外波段的光转化为可见光,具有高透光率、耐老化、无黄变、柔软性的特性,常用液态硅胶固化后形成的第一透光胶膜和第二透光胶膜即可达到玻璃94%左右的透光率,可以实现对光照的充分利用。
参考表1,本实施例提供的太阳能电池组件的制备方法可以有效提高太阳能电池组件的阻水性和太阳能电池组件的光学增益,还可以提高太阳能电池组件的可靠性和功率,经模拟测试,结果表明可以将太阳能电池组件的使用寿命延长至40年以上。表1中为分别对两组本实施例提供的太阳能电池组件进行不同测试项目,并获得不同的测试参数。其中,“初始”指的是对太阳能电池组件不做任何处理进行电学性能参数的测试;“DH1000h”指的是对太阳能电池组件进行湿热老化实验1000小时之后进行电学性能参数的测试,“DH1000h”衰减”指的对太阳能电池组件进行湿热老化测试1000小时之后与对太阳能电池组件不做任何处理之后相比电学性能参数的变化;“TC200”指的是对太阳能电池组件进行温度循环,总共做了200次循环之后进行电学性能参数的测试,“TC200衰减”指的是对太阳能电池组件进行温度循环200次之后与对太阳能电池组件不做任何处理之后的电学性能参数的变化;“PID288h”指的是对太阳能电池组件进行288小时电势诱导衰减之后进行电学性能参数的测试,“PID288h衰减”指的是对太阳能电池组件进行288小时电势诱导衰减之后与对太阳能电池组件不做任何处理之后的电学性能参数的变化;“UV120”是对太阳能电池组件进行紫外照射,照射的功率为120kWh之后进行电学性能参数的测试,“UV120衰减”是对太阳能电池组件进行紫外照射,照射的功率为120kWh之后与对太阳能电池组件不做任何处理之后的
电学性能参数的变化。测试参数中,Isc指的是短路电流,Voc指的是开路电压,Imp指的是最大功率点的电流,Vmp指的是最大功率点的电压,Pmax指的是最大功率温度系数,FF指的是填充因子。
表1
表1中的测试数据,为按照IEC测试标准进行环境老化类实验,从“DH1000h衰减”、“TC200衰减”、“PID288h衰减”以及“UV120衰减”的参数可以看出,采用本实施例提供的太阳能电池组件的制备方法形成的太阳能电池组件,实验结果表明,太阳能电池组件的功率衰减远远小于IEC测试要求标准,由此可以看出该太阳能电池组件的制备方法形成的太阳能电池组件具有优异的抗老化性能,能显著增加该电池组件的可靠性。
参考表2,表2为采用本实施例提供的太阳能电池组件的制备方法形成的太阳能电池组件的短路电流参数与采用常规高透胶膜封装形成的太阳能电池组件的光谱响应的电流积分密度,可以看出,常规高透胶膜封装形成的太阳能电池组件与采用本实施例提供的太阳能电池组件的制备方法形成的太阳能电池组件相比,本实施例提供的太阳能电池组件的制备方法形成的太阳能电池组件在
300nm-1200nm范围的光谱,光电转换效率提升了1.4%,在300nm-380nm范围的光谱,光电转换效率提升了2.5%,在380nm-780nm范围的光谱,光电转换效率提升了1.3%,在780nm-1200nm范围的光谱,光电转换效率提升了1.5%。从整体上提升了组件的功率。
表2
参考图10,图10为采用本实施例提供的太阳能电池组件的制备方法形成的太阳能电池组件与采用常规高透胶膜封装形成的太阳能电池组件的光谱响应对比图,图10中横坐标代表的是波长,纵坐标代表的是光谱响应,光谱响应表示太阳能电池对不同波长入射光能转换成电能的能力,其单位为安培/瓦(Amp/Watt)。从图10可以看出,在紫外波段400nm~1080nm,采用本实施例提供的太阳能电池组件的制备方法形成的太阳能电池组件的内量子效率明显优于采用常规高透胶膜封装形成的太阳能电池组件,更直观地反应出本实施例提供的太阳能电池组件的制备方法形成的太阳能电池组件光电转换效率优于采用常规高透胶膜封装形成的太阳能电池组件。
显然,上述实施例仅仅是为清楚地说明所作的举例,而并非对实施方式的限定。对于所属领域的普通技术人员来说,在上述说明的基础上还可以做出其它不同形式的变化或变动。这里无需也无法对所有的实施方式予以穷举。而由此所引伸出的显而易见的变化或变动仍处于本发明创造的保护范围之中。
Claims (10)
- 一种太阳能电池组件的制备方法,其特征在于,包括:提供第一封装层,所述第一封装层包括电池组放置区和环绕所述电池组放置区的边缘区;在所述第一封装层的一侧的边缘区形成阻水胶层;在所述第一封装层的一侧的电池组放置区形成液态或半液半固态的第一透光胶膜,所述第一透光胶膜与所述阻水胶层位于所述第一封装层的同侧;在所述第一透光胶膜背离所述第一封装层的一侧表面铺设太阳能电池组;在所述太阳能电池组背离所述第一透光胶膜的一侧表面形成液态或半液半固态的第二透光胶膜;在所述阻水胶层和所述第二透光胶膜背离所述第一封装层的一侧设置第二封装层,所述阻水胶层的厚度等于或者大于所述第二透光胶膜背离所述第一封装层一侧表面至所述第一封装层的距离;对包括所述第一封装层、所述第一透光胶膜、所述太阳能电池组、所述第二透光胶膜和所述第二封装层的结构进行层压,层压后使得所述第一透光胶膜和所述第二透光胶膜熔融后固化,所述第一透光胶膜和所述第二透光胶膜均与所述阻水胶层接触。
- 根据权利要求1所述的太阳能电池组件的制备方法,其特征在于,在所述第一封装层的一侧的电池组放置区形成液态或半液半固态的第一透光胶膜的步骤中,所述第一透光胶膜和所述阻水胶层之间具有间隙;对所述第一封装层、所述第一透光胶膜、所述太阳能电池组、所述第二透光胶膜和所述第二封装层进行层压的步骤中,所述第一透光胶膜和/或第二透光胶膜填充所述间隙;优选的,所述间隙的宽度尺寸为2mm~8mm;优选的,所述阻水胶层的厚度比所述第二透光胶膜背离所述第一封装层一侧表面至所述第一封装层的距离大0.2mm~0.5mm。
- 根据权利要求1所述的太阳能电池组件的制备方法,其特征在于,液态或半液半固态的第一透光胶膜的粘稠度为40000mpa.s~60000mpa.s;液态或半液半固态的第二透光胶膜的粘稠度为40000mpa.s~60000mpa.s。
- 根据权利要求1所述的太阳能电池组件的制备方法,其特征在于,形成液态或半液半固态的第一透光胶膜采用的工艺包括喷涂工艺或丝网印刷工艺;形成 液态或半液半固态第二透光胶膜采用的工艺包括喷涂工艺或丝网印刷工艺。
- 根据权利要求4所述的太阳能电池组件的制备方法,其特征在于,形成液态或半液半固态的第一透光胶膜采用的工艺包括喷涂工艺;形成液态或半液半固态的第一透光胶膜的步骤中:沿着第一方向和第二方向交错进行喷涂;所述第一方向与第二方向垂直;形成液态或半液半固态的第二透光胶膜采用的工艺包括喷涂工艺;形成液态或半液半固态的第二透光胶膜的步骤中:沿着第一方向和第二方向交错进行喷涂;所述第一方向与第二方向垂直。
- 根据权利要求1所述的太阳能电池组件的制备方法,其特征在于,对所述第一封装层、所述第一透光胶膜、所述太阳能电池组、所述第二透光胶膜和所述第二封装层进行层压的参数包括:层压的温度为:70℃~120℃;层压的时间为:660s~700s,层压的压强为35kPa~75kPa;优选的,对所述第一封装层、所述第一透光胶膜、所述太阳能电池组、所述第二透光胶膜和所述第二封装层进行层压的过程包括:依次进行的第一次层压、第二次层压和第三次层压,第一次层压、第二次层压和第三次层压的压强递减;优选的,第一次层压的压强为65kPa~75kPa;第二次层压的压强为45kPa~55kPa;第三次层压的压强为35kPa~45kPa;优选的,第一次层压的时间为15s~25s;第二次层压的时间为15s~25s;第三次层压的时间为630s~650s。
- 根据权利要求1~6任一项所述的太阳能电池组件的制备方法,其特征在于,在所述第一封装层的一侧的电池组放置区形成液态或半液半固态的第一透光胶膜的步骤中,所述第一透光胶膜的厚度为0.3mm~0.8mm;在所述太阳能电池组背离所述第一透光胶膜的一侧表面形成液态或半液半固态的第二透光胶膜的步骤中,所述第二透光胶膜的厚度为0.3mm~0.8mm。
- 根据权利要求1~6任一项所述的太阳能电池组件的制备方法,其特征在于,所述第一透光胶膜的材料包括液态硅胶、硅胶、液态硅橡胶、液态胶、凝胶、有机硅凝胶、硅体胶、硅橡胶、液态原料、硅橡胶胶料和硅橡胶原料中的至少一种;所述第二透光胶膜的材料包括液态硅胶、硅胶、液态硅橡胶、液态胶、凝胶、有机硅凝胶、硅体胶、硅橡胶、液态原料、硅橡胶胶料和硅橡胶原料中的至少一种。
- 根据权利要求1~6任一项所述的太阳能电池组件的制备方法,其特征在于,对所述第一封装层、所述第一透光胶膜、所述太阳能电池组、所述第二透光胶膜和所述第二封装层进行层压之前,所述阻水胶层的宽度为2mm~15mm,所述阻水胶层的厚度为0.5mm~3.5mm。
- 根据权利要求1~6任一项所述的太阳能电池组件的制备方法,其特征在于,所述阻水胶层的材料包括异丁烯类聚合物、异戊二烯类聚合物中的任意一种。