WO2023051693A1 - Nitrogen dopant feeding apparatus and method, and system for manufacturing nitrogen-doped monocrystalline silicon rod - Google Patents

Nitrogen dopant feeding apparatus and method, and system for manufacturing nitrogen-doped monocrystalline silicon rod Download PDF

Info

Publication number
WO2023051693A1
WO2023051693A1 PCT/CN2022/122591 CN2022122591W WO2023051693A1 WO 2023051693 A1 WO2023051693 A1 WO 2023051693A1 CN 2022122591 W CN2022122591 W CN 2022122591W WO 2023051693 A1 WO2023051693 A1 WO 2023051693A1
Authority
WO
WIPO (PCT)
Prior art keywords
nitrogen
silicon nitride
melt
silicon
feeding device
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Ceased
Application number
PCT/CN2022/122591
Other languages
French (fr)
Chinese (zh)
Inventor
徐鹏
衡鹏
李阳
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Xian Eswin Material Technology Co Ltd
Original Assignee
Xian Eswin Material Technology Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Xian Eswin Material Technology Co Ltd filed Critical Xian Eswin Material Technology Co Ltd
Publication of WO2023051693A1 publication Critical patent/WO2023051693A1/en
Anticipated expiration legal-status Critical
Ceased legal-status Critical Current

Abstract

A nitrogen dopant feeding apparatus and method, and a system for manufacturing a nitrogen-doped monocrystalline silicon rod. The nitrogen dopant feeding apparatus comprises: a carrier tube provided with an opening at the bottom, and a heating apparatus surrounding the outer side of the carrier tube; a blocking apparatus provided inside the carrier tube, the blocking device being able to fit with the bottom of the carrier tube to shield the opening, and a gap being able to be formed between the blocking apparatus and the bottom of the carrier tube to open the opening; and a lifting/lowering mechanism, the lifting/lowering mechanism being configured to lift or lower the blocking apparatus.

Description

氮掺杂剂加料装置、方法及氮掺杂单晶硅棒的制造系统Nitrogen dopant feeding device, method and manufacturing system of nitrogen-doped single crystal silicon rod

相关申请的交叉引用Cross References to Related Applications

本申请主张在2021年9月29日在中国提交的中国专利申请No.202111152860.3的优先权,其全部内容通过引用包含于此。This application claims priority to Chinese Patent Application No. 202111152860.3 filed in China on September 29, 2021, the entire contents of which are hereby incorporated by reference.

技术领域technical field

本申请实施例涉及半导体技术领域,尤其涉及一种氮掺杂剂加料装置、方法及氮掺杂单晶硅棒的制造系统。The embodiments of the present application relate to the field of semiconductor technology, and in particular to a nitrogen dopant feeding device and method, and a manufacturing system for nitrogen-doped single crystal silicon rods.

背景技术Background technique

用于生产集成电路(Integrated Circuit,IC)等半导体电子元器件的硅片,主要通过将直拉(Czochralski)法拉制的单晶硅棒切片而制造出。Czochralski法包括使由石英制成的坩埚中的多晶硅原料熔化以获得硅熔体,将籽晶晶种浸入硅熔体中,以及连续地提升籽晶晶种移动离开硅熔体表面,由此在移动过程中在相界面处生长出单晶硅棒。Silicon wafers for the production of semiconductor electronic components such as integrated circuits (Integrated Circuit, IC), are mainly manufactured by slicing single crystal silicon rods drawn by the Czochralski method. The Czochralski method involves melting polysilicon raw material in a crucible made of quartz to obtain a silicon melt, immersing a seed crystal in the silicon melt, and continuously lifting the seed crystal to move away from the surface of the silicon melt, thereby During the movement, single crystal silicon rods are grown at the phase interface.

在上述生产过程中,生产制造一种无位错,甚至无孪晶以及无多晶的单晶硅棒是非常有利的,这种单晶硅棒具有良好的机械性能以及优良的电特性。而目前生产这种单晶硅棒的其中之一的方法就是在硅熔体中掺杂氮原子,以通过氮原子起到钉扎位错的作用,这主要是因为氮掺杂的单晶硅棒的位错移动激活能比无掺杂的单晶硅棒的位错移动激活能高,进而使得氮掺杂的单晶硅棒的位错滑移的距离短,因此在单晶硅棒中掺杂氮能够抑制位错,甚至孪晶和多晶的产生。目前,作为氮掺杂的一种实现方式,可以在石英坩埚中的硅熔体中掺杂氮,由此拉制出的单晶硅棒以及由单晶硅棒切割出的硅片中便会掺杂有氮。In the above-mentioned production process, it is very advantageous to produce a dislocation-free, even twin-free and polycrystalline single-crystal silicon rod, which has good mechanical properties and excellent electrical properties. One of the current methods of producing this single crystal silicon rod is to dope nitrogen atoms in the silicon melt, so as to play the role of pinning dislocations through nitrogen atoms. This is mainly because nitrogen-doped single crystal silicon The dislocation movement activation energy of the rod is higher than that of the undoped single crystal silicon rod, which makes the dislocation slip distance of the nitrogen-doped single crystal silicon rod shorter, so in the single crystal silicon rod Nitrogen doping can suppress dislocations, and even the generation of twins and polycrystals. At present, as a way to realize nitrogen doping, nitrogen can be doped in the silicon melt in the quartz crucible, and the single crystal silicon rods drawn from this and the silicon wafers cut from the single crystal silicon rods will be Doped with nitrogen.

目前,氮掺杂的技术一般使用氮化硅(Si 3N 4)作为氮源,片状或颗粒状氮化硅材料投入到多晶硅原料中,实现氮元素的加入,但是由于氮化硅熔化温度(约1800℃)比硅熔点(1425℃)高,需要加热并稳定一段时间的高温(大于1600℃)后才能使其完全熔融在硅熔体中,而单晶硅棒拉制时硅熔体 中不能存在未熔化的氮化硅微粒,否则该氮化硅微粒会进入单晶硅棒中造成单晶硅棒内产生位错,进而导致单晶硅棒产品的报废;而且太高的氮化硅熔体温度也会容易造成石英坩埚软化加剧,致使SiO 2中的析出氧增加,以使得单晶硅棒拉制过程中的氧含量难以控制,从而使得单晶硅棒顶部的氧含量偏高,影响单晶硅棒的产品品质。 At present, the technology of nitrogen doping generally uses silicon nitride (Si 3 N 4 ) as the nitrogen source, and the flake or granular silicon nitride material is put into the polysilicon raw material to realize the addition of nitrogen element, but due to the melting temperature of silicon nitride (about 1800°C) is higher than the melting point of silicon (1425°C), and it needs to be heated and stabilized at a high temperature (greater than 1600°C) for a period of time before it can be completely melted in the silicon melt, while the silicon melt is melted when the single crystal silicon rod is drawn There should be no unmelted silicon nitride particles in the film, otherwise the silicon nitride particles will enter the single crystal silicon rod and cause dislocations in the single crystal silicon rod, which will lead to the scrapping of the single crystal silicon rod product; The temperature of the silicon melt will also easily cause the softening of the quartz crucible to increase, resulting in an increase in the precipitated oxygen in SiO 2 , making it difficult to control the oxygen content during the drawing process of the single crystal silicon rod, resulting in a high oxygen content at the top of the single crystal silicon rod , affecting the product quality of monocrystalline silicon rods.

此外,尤其在拉制含氮掺杂和其他掺杂剂例如硼的单晶硅棒时,硅熔体温度太高会造成掺杂剂硼的挥发量增加,更严重地将导致硼原子与氮原子在超过1600℃的高温下形成难熔物氮化硼,该氮化硼物质在硅熔体中一直存在,易造成单晶硅棒产生位错、孪晶甚至多晶,进而导致单晶硅棒产品的报废。In addition, especially when drawing single crystal silicon rods containing nitrogen doped and other dopants such as boron, too high temperature of silicon melt will cause the volatilization of dopant boron to increase, and more seriously will cause boron atoms to interact with nitrogen Atoms form refractory boron nitride at a high temperature of more than 1600 ° C. This boron nitride substance always exists in the silicon melt, which is easy to cause dislocation, twinning and even polycrystals in single crystal silicon rods, which in turn leads to single crystal silicon Scrapping of stick products.

发明内容Contents of the invention

有鉴于此,本申请实施例期望提供一种氮掺杂剂加料装置、方法及氮掺杂单晶硅棒的制造系统;能够获得无位错、无孪晶以及无多晶的高品质的氮掺杂单晶硅棒。In view of this, the embodiment of the present application expects to provide a nitrogen dopant feeding device, method, and manufacturing system for nitrogen-doped single crystal silicon rods; it is possible to obtain high-quality nitrogen without dislocations, twins, and polycrystals. Doped monocrystalline silicon rods.

本申请实施例的技术方案是这样实现的:The technical scheme of the embodiment of the application is realized in this way:

第一方面,本申请实施例提供了一种氮掺杂剂加料装置,所述氮掺杂剂加料装置设置于石英坩埚的正上方,所述氮掺杂剂加料装置包括:In the first aspect, the embodiment of the present application provides a nitrogen dopant feeding device, the nitrogen dopant feeding device is arranged directly above the quartz crucible, and the nitrogen dopant feeding device includes:

底部设置有开口的承载管,所述承载管用于承载待熔化的氮化硅;A carrying tube with an opening at the bottom, the carrying tube is used to carry the silicon nitride to be melted;

环绕于所述承载管外侧的加热装置,所述加热装置用于加热所述待熔化的氮化硅使其完全熔化成氮化硅熔体;a heating device surrounding the outside of the carrying tube, the heating device is used to heat the silicon nitride to be melted to completely melt it into a silicon nitride melt;

设置于所述承载管内部的隔挡装置,所述隔挡装置能够与所述承载管的底部贴合以遮挡所述开口,以防止所述待熔化的氮化硅从所述开口处掉落至所述石英坩埚中;以及,所述隔挡装置能够与所述承载管的底部产生间隙以打开所述开口,以使得所述氮化硅熔体从所述开口处滴落至承载有含硼原子的硅熔体的所述石英坩埚中;A blocking device arranged inside the carrying tube, the blocking device can be attached to the bottom of the carrying tube to cover the opening, so as to prevent the silicon nitride to be melted from falling from the opening into the quartz crucible; and, the barrier device can create a gap with the bottom of the carrier tube to open the opening, so that the silicon nitride melt drips from the opening to the carrier containing silicon melt of boron atoms in said quartz crucible;

升降机构,所述升降机构用于提升或下降所述隔挡装置。A lifting mechanism, the lifting mechanism is used to lift or lower the blocking device.

第二方面,本申请实施例提供了一种氮掺杂剂加料方法,所述氮掺杂剂加料方法能够应用于第一方面所述的氮掺杂剂加料装置中,所述氮掺杂剂加料方法包括:In the second aspect, the embodiment of the present application provides a nitrogen dopant feeding method, the nitrogen dopant feeding method can be applied to the nitrogen dopant feeding device described in the first aspect, the nitrogen dopant Feeding methods include:

将多晶硅原料及硼掺杂剂放置于石英坩埚中并升温至1450℃以使得所述多晶硅原料及所述硼掺杂剂熔化形成含硼原子的硅熔体;placing the polysilicon raw material and the boron dopant in a quartz crucible and raising the temperature to 1450° C. to melt the polysilicon raw material and the boron dopant to form a silicon melt containing boron atoms;

将设定质量的待熔化的氮化硅投入至氮掺杂剂加料装置中,并通过加热装置升温至1800℃以使得所述待熔化的氮化硅熔化形成氮化硅熔体;Putting a set mass of silicon nitride to be melted into the nitrogen dopant feeding device, and raising the temperature to 1800° C. through a heating device so that the silicon nitride to be melted is melted to form a silicon nitride melt;

通过升降机构提升隔挡装置,以使得所述氮化硅熔体通过承载管底部的开口滴落至所述含硼原子的硅熔体中。The barrier device is lifted by the lifting mechanism, so that the silicon nitride melt drops into the silicon melt containing boron atoms through the opening at the bottom of the supporting tube.

第三方面,本申请实施例提供了一种氮掺杂单晶硅棒的制造系统,所述制造系统包括:根据第一方面所述的氮掺杂剂加料装置,以及拉晶设备;其中,In a third aspect, an embodiment of the present application provides a manufacturing system for nitrogen-doped single crystal silicon rods, the manufacturing system includes: the nitrogen dopant feeding device according to the first aspect, and crystal pulling equipment; wherein,

所述氮掺杂剂加料装置用于将氮化硅熔体掺入所述拉晶设备中石英坩埚内的含硼原子的硅熔体中;The nitrogen dopant feeding device is used to mix the silicon nitride melt into the silicon melt containing boron atoms in the quartz crucible in the crystal pulling equipment;

所述拉晶设备用于利用含氮原子和硼原子的硅熔体采用Czochralski法拉制单晶硅棒。The crystal pulling equipment is used for pulling single crystal silicon rods by using the silicon melt containing nitrogen atoms and boron atoms by Czochralski method.

本申请实施例提供了一种氮掺杂剂加料装置、方法及氮掺杂单晶硅棒的制造系统;在该氮掺杂剂加料装置中,在待熔化的氮化硅投入承载管之前,先通过升降机构下降隔挡装置与承载管底部贴合以遮挡开口,以防止待熔化的氮化硅从开口处掉落至石英坩埚中;当待熔化的氮化硅完全熔化成氮化硅熔体后,利用升降机构提升隔挡装置以打开开口,从而使得氮化硅熔体滴落至含硼原子的硅熔体中;利用该氮掺杂剂加料装置能够将氮化硅熔体加入至含硼原子的硅熔体中,这样石英坩埚内形成含硼原子的硅熔体的温度无需超过1600℃,而在含硼原子的硅熔体的熔化温度不超过1600℃的情况下,氮化硅熔体中的氮原子即可掺入含硼原子的硅熔体中,因此在整个单晶硅棒拉制过程中不会产生氮化硼颗粒,进而最终形成的单晶硅棒中也不会产生位错,甚至孪晶以及多晶缺陷。The embodiment of the present application provides a nitrogen dopant feeding device, method, and manufacturing system for nitrogen-doped single crystal silicon rods; in the nitrogen dopant feeding device, before the silicon nitride to be melted is put into the carrier tube, Firstly, the lifting mechanism is used to lower the blocking device to fit the bottom of the carrying tube to cover the opening, so as to prevent the silicon nitride to be melted from falling into the quartz crucible from the opening; when the silicon nitride to be melted is completely melted into a silicon nitride melt After solidification, use the lifting mechanism to lift the blocking device to open the opening, so that the silicon nitride melt drops into the silicon melt containing boron atoms; the silicon nitride melt can be added to the silicon nitride melt by using the nitrogen dopant feeding device In the silicon melt containing boron atoms, the temperature of the silicon melt containing boron atoms in the quartz crucible does not need to exceed 1600°C, and when the melting temperature of the silicon melt containing boron atoms does not exceed 1600°C, nitriding The nitrogen atoms in the silicon melt can be incorporated into the silicon melt containing boron atoms, so boron nitride particles will not be produced during the entire drawing process of the single crystal silicon rod, and there will be no boron nitride particles in the final formed single crystal silicon rod. Dislocations, even twins, and polycrystalline defects will occur.

附图说明Description of drawings

图1为本申请实施例提供的常规技术方案中氮掺杂的一种实现方式的示意图;Figure 1 is a schematic diagram of an implementation of nitrogen doping in the conventional technical solution provided by the embodiment of the present application;

图2为本申请实施例提供的硅熔体中生成有氮化硼的示意图;Fig. 2 is the schematic diagram that boron nitride is generated in the silicon melt provided by the embodiment of the present application;

图3为本申请实施例提供的一种氮掺杂剂加料装置的示意图;FIG. 3 is a schematic diagram of a nitrogen dopant feeding device provided in an embodiment of the present application;

图4为本申请实施例提供的利用氮掺杂剂加料装置实现硅熔体中氮掺杂的示意图;Fig. 4 is a schematic diagram of nitrogen doping in silicon melt realized by using a nitrogen dopant feeding device provided in an embodiment of the present application;

图5为本申请实施例提供的一种氮掺杂剂加料方法的流程示意图;Fig. 5 is a schematic flow chart of a nitrogen dopant feeding method provided in the embodiment of the present application;

图6为本申请实施例提供的一种氮掺杂单晶硅棒的制造系统。FIG. 6 is a manufacturing system for a nitrogen-doped single crystal silicon rod provided in an embodiment of the present application.

具体实施方式Detailed ways

下面将结合本申请实施例中的附图,对本申请实施例中的技术方案进行清楚、完整地描述。The technical solutions in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application.

参见图1,其示出了常规技术方案中氮掺杂的一种实现方式。如图1所示,多晶硅原料B1和其他掺杂剂例如硼B2与氮化硅B3一起容纳在石英坩埚QC中,其中,多晶硅原料B1通过由线框围绕的区域示意性地示出,硼掺杂剂B2通过由斜线填充的区域示意性地示出,氮化硅B3通过由黑色填充区域示意性地示出。当对石英坩埚QC进行加热使容纳在石英坩埚QC中的多晶硅原料B1、硼掺杂剂B2以及氮化硅B3熔化后,便可以获得包括包含硅原子、硼原子和氮原子的熔体M。但是,在上述实现方式中,由于氮化硅B3的熔化温度约为1800℃,而多晶硅原料B1和硼掺杂剂B2的熔化温度不能超过1600℃,因此来自于氮化硅B3的氮原子无法获得足够充分地熔解,而是仅能够熔解在每个氮化硅B3周围的一定范围内,因此掺杂的氮在熔体M整体中的分布是不均匀的。具体地,参见图1,所获得的熔体M按照氮浓度或含氮量的不同仍然大致可以分为如下的三种区域:含氮量低的第一熔体区域M1,如在图1中通过低密度的点填充的区域示意性地示出的,该区域在石英坩埚QC中处于与氮化硅B3的几何中心相距远距离的位置处;含氮量中等的第二熔体区域M2,如在图1中通过中等密度的点填充的区域示意性地示出的,该区域在石英坩埚QC中处于与氮化硅B3的几何中心相距中等距离的位置处;含氮量高的第三熔体区域M3,如在图1中通过高密度的点填充的区域示意性地示出的,该区域在石英坩埚QC中处于与氮化硅B3的几何中心相距近距离的位置处。Referring to FIG. 1 , it shows an implementation of nitrogen doping in conventional technical solutions. As shown in Figure 1, polysilicon raw material B1 and other dopants such as boron B2 are housed in a quartz crucible QC together with silicon nitride B3, wherein polysilicon raw material B1 is schematically shown by the area surrounded by a wire frame, boron doped The dopant B2 is schematically indicated by the area filled with oblique lines, and the silicon nitride B3 is schematically indicated by the area filled with black. After the quartz crucible QC is heated to melt the polysilicon raw material B1, boron dopant B2 and silicon nitride B3 contained in the quartz crucible QC, a melt M containing silicon atoms, boron atoms and nitrogen atoms can be obtained. However, in the above implementation, since the melting temperature of silicon nitride B3 is about 1800°C, and the melting temperature of polysilicon raw material B1 and boron dopant B2 cannot exceed 1600°C, nitrogen atoms from silicon nitride B3 cannot Melting is sufficiently complete, but can only be melted within a certain range around each silicon nitride B3, so that the distribution of doped nitrogen in the melt M as a whole is not uniform. Specifically, referring to Fig. 1, the obtained melt M can be roughly divided into the following three regions according to the difference in nitrogen concentration or nitrogen content: the first melt region M1 with low nitrogen content, as shown in Fig. 1 Schematically shown by a low-density point-filled region at a distance from the geometric center of the silicon nitride B3 in the quartz crucible QC; the second melt region M2 with a moderate nitrogen content, As shown schematically in Fig. 1 by the dot-filled region of moderate density, this region is at a moderate distance from the geometric center of the silicon nitride B3 in the quartz crucible QC; the nitrogen-rich third The melt region M3 , which is schematically shown in FIG. 1 by a region filled with high density of points, is located at a short distance from the geometric center of the silicon nitride B3 in the quartz crucible QC.

需要说明的是,前述氮化硅B3的形状不限于片状、也可以是颗粒状。It should be noted that the shape of the aforementioned silicon nitride B3 is not limited to a flake shape, and may also be a granular shape.

另一方面,如若为了完全地熔解氮化硅B3,将多晶硅原料B1和硼掺杂剂B2的熔化温度升高至1600℃以上,此时熔体M中则会形成氮化硼颗粒B4,具体如图2中的黑色圆形所示。由于氮化硼颗粒B4为难熔物,会一直存在于熔体M内,易造成单晶硅棒中产生位错、孪晶甚至多晶的缺陷,严重时将导致单晶硅棒产品报废。On the other hand, if in order to completely melt silicon nitride B3, the melting temperature of polysilicon raw material B1 and boron dopant B2 is raised above 1600°C, boron nitride particles B4 will be formed in the melt M at this time, specifically It is shown as a black circle in Figure 2. Since the boron nitride particle B4 is a refractory material, it will always exist in the melt M, which may easily cause dislocation, twinning or even polycrystalline defects in the single crystal silicon rod, and in severe cases, the single crystal silicon rod product will be scrapped.

基于上述阐述,为了获得无位错、无孪晶以及无多晶缺陷的含氮原子和硼原子的单晶硅棒,本申请实施例期望在能够获得含硼原子的硅熔体M'的基础上,改进氮化硅B3的加料方式。图3为本申请实施例提供的一种氮掺杂剂加料装置30的示意图,其中,氮掺杂剂加料装置30设置于石英坩埚QC的正上方,所述氮掺杂剂加料装置30具体可以包括:Based on the above description, in order to obtain a single crystal silicon rod containing nitrogen atoms and boron atoms without dislocations, twins, and polycrystalline defects, the embodiment of the present application expects to obtain silicon melt M' containing boron atoms Above, improve the feeding method of silicon nitride B3. Fig. 3 is a schematic diagram of a nitrogen dopant feeding device 30 provided in the embodiment of the present application, wherein the nitrogen dopant feeding device 30 is arranged directly above the quartz crucible QC, and the nitrogen dopant feeding device 30 can specifically be include:

底部设置有开口3011的承载管301,所述承载管301用于承载待熔化的氮化硅B3;The bottom is provided with a carrying tube 301 with an opening 3011, and the carrying tube 301 is used to carry the silicon nitride B3 to be melted;

环绕于所述承载管外侧的加热装置302,所述加热装置302用于加热所述待熔化的氮化硅B3使其完全熔化成氮化硅熔体M";A heating device 302 surrounding the outside of the carrying tube, the heating device 302 is used to heat the silicon nitride B3 to be melted so that it is completely melted into a silicon nitride melt M";

设置于所述承载管内部的隔挡装置303,所述隔挡装置303能够与所述承载管301的底部贴合以遮挡所述开口3011,以防止所述待熔化的氮化硅B3从所述开口3011处掉落至所述石英坩埚QC中;以及,所述隔挡装置303能够与所述承载管301的底部产生间隙以打开所述开口3011,以使得所述氮化硅熔体M"从所述开口3011处滴落至承载有含硼原子的硅熔体M'的所述石英坩埚QC中;The blocking device 303 arranged inside the carrying tube, the blocking device 303 can be attached to the bottom of the carrying tube 301 to block the opening 3011, so as to prevent the silicon nitride B3 to be melted from the drop into the quartz crucible QC at the opening 3011; "dropping from the opening 3011 into the quartz crucible QC carrying the silicon melt M' containing boron atoms;

升降机构304,所述升降机构304用于提升或下降所述隔挡装置303。The lifting mechanism 304 is used for lifting or lowering the blocking device 303 .

可以理解地,对于根据本申请的氮掺杂剂加料装置30而言,如图3中所示,在待熔化的氮化硅B3放置在氮掺杂剂加料装置30之前,先通过升降机构304下降隔挡装置与承载管301底部贴合以遮挡开口3011,以防止待熔化的氮化硅B3从开口3011处掉落至石英坩埚QC中;而如图4所示,当待熔化的氮化硅B3完全熔化成氮化硅熔体M"后,利用升降机构304提升隔挡装置303以打开开口3011,从而使得氮化硅熔体M"滴落至含硼原子的硅熔体M'中。It can be understood that, for the nitrogen dopant feeding device 30 according to the present application, as shown in FIG. The descending blocking device fits with the bottom of the carrier tube 301 to block the opening 3011, so as to prevent the silicon nitride B3 to be melted from falling into the quartz crucible QC from the opening 3011; and as shown in Figure 4, when the silicon nitride B3 to be melted After the silicon B3 is completely melted into a silicon nitride melt M", the lifting mechanism 304 is used to lift the blocking device 303 to open the opening 3011, so that the silicon nitride melt M" drops into the silicon melt M' containing boron atoms .

利用该氮掺杂剂加料装置30能够将氮化硅熔体M"加入至含硼原子的硅 熔体M'中,这样石英坩埚QC内形成含硼原子的硅熔体M'的温度无需超过1600℃,而在含硼原子的硅熔体M'的熔化温度不超过1600℃的情况下,氮化硅熔体M"中的氮原子即可掺入含硼原子的硅熔体M'中,因此在整个单晶硅棒的拉制过程中不会产生氮化硼颗粒B4,进而最终形成的单晶硅棒中也不会产生位错,甚至孪晶以及多晶缺陷。Utilize this nitrogen dopant feeding device 30 to be able to add silicon nitride melt M " in the silicon melt M ' that contains boron atom, the temperature that forms the silicon melt M ' that contains boron atom in the quartz crucible QC like this need not exceed 1600°C, and when the melting temperature of the silicon melt M' containing boron atoms does not exceed 1600°C, the nitrogen atoms in the silicon nitride melt M" can be incorporated into the silicon melt M' containing boron atoms , so boron nitride particles B4 will not be generated during the entire pulling process of the single crystal silicon rod, and then no dislocations, even twins and polycrystalline defects will be generated in the final formed single crystal silicon rod.

此外,可以理解地,采用氮化硅熔体M"加入至含硼原子的硅熔体M'的方法,不会造成石英坩埚QC内的最终温度过高,因而不会容易造成石英坩埚QC软化加剧,以致使SiO 2中的析出氧增加,因此也就不会在单晶硅棒拉制过程中出现氧含量难以控制的现象。 In addition, it can be understood that the method of adding the silicon nitride melt M" to the silicon melt M' containing boron atoms will not cause the final temperature in the quartz crucible QC to be too high, and thus will not easily cause the quartz crucible QC to soften. Intensified, so that the precipitated oxygen in SiO 2 increases, so there will be no phenomenon that the oxygen content is difficult to control during the drawing process of single crystal silicon rods.

需要说明的是,承载管301中放置的待熔化的氮化硅B3的质量是预先设定的,以保证最终拉制的单晶硅棒中的氮含量满足产品要求。It should be noted that the quality of the silicon nitride B3 to be melted placed in the carrier tube 301 is preset to ensure that the nitrogen content in the finally drawn single crystal silicon rod meets the product requirements.

对于图3所示的氮掺杂剂加料装置30,在一些示例中,所述承载管301的材料为高密度氮化硅。可以理解地,当待熔化的氮化硅B3升温熔化时,整个氮掺杂剂加料装置30内部的整体温度会升温至1800℃,因此为了保证承载管301的使用寿命,承载管301需要使用耐高温材料;而另一方面为了保证待熔化的氮化硅B3在升温熔化的过程中不会引入新的杂质,因此可选地,承载管301的材料为高密度氮化硅材料。For the nitrogen dopant feeding device 30 shown in FIG. 3 , in some examples, the material of the carrying tube 301 is high-density silicon nitride. It can be understood that when the silicon nitride B3 to be melted is heated and melted, the overall temperature inside the nitrogen dopant feeding device 30 will rise to 1800° C. High-temperature material; on the other hand, in order to ensure that the silicon nitride B3 to be melted will not introduce new impurities during the process of heating and melting, therefore, optionally, the material of the carrying tube 301 is a high-density silicon nitride material.

对于图3所示的氮掺杂剂加料装置30,在一些示例中,可选地,所述加热装置为电阻式加热器。这主要是因为利用电阻式加热器对承载管301加热时能够精确地控制待熔化的氮化硅B3的熔化温度;其次,利用电阻式加热器加热时承载管301受热均匀,因而待熔化的氮化硅B3能够得到均匀地熔解。当然,可以理解地,电阻式加热器的热效率高,对承载管301加热升温时热损失少,能够有效地节省加热成本。For the nitrogen dopant feeding device 30 shown in FIG. 3 , in some examples, optionally, the heating device is a resistance heater. This is mainly because the melting temperature of the silicon nitride B3 to be melted can be precisely controlled when the resistance heater is used to heat the carrier tube 301; secondly, the carrier tube 301 is heated evenly when the resistance heater is used for heating, so the nitrogen to be melted SiC B3 can be melted uniformly. Of course, it can be understood that the thermal efficiency of the resistance heater is high, and the heat loss is small when heating the carrying tube 301 to raise the temperature, which can effectively save the heating cost.

对于图3所示的氮掺杂剂加料装置30,在一些示例中,可选地,所述隔挡装置303包括连动杆3031和隔挡球3032;其中,所述连动杆3031和所述隔挡球3032固定连接。需要说明的是,连动杆3031和隔挡球3032可以采用焊接的方式固定地连接在一起,也可以在具体实施过程中将连动杆3031和隔挡球3032制造为一体结构。For the nitrogen dopant feeding device 30 shown in FIG. 3 , in some examples, optionally, the barrier device 303 includes a linkage rod 3031 and a barrier ball 3032; wherein, the linkage rod 3031 and the barrier ball 3032 The barrier ball 3032 is fixedly connected. It should be noted that the linkage rod 3031 and the barrier ball 3032 can be fixedly connected together by welding, or the linkage rod 3031 and the barrier ball 3032 can be manufactured as an integrated structure during the specific implementation process.

对于上述示例,在一些具体的实施方式中,可选地,所述连动杆3031和 所述隔挡球3032的材料为高密度氮化硅。可以理解地,在待熔化的氮化硅B3升温熔化的过程中,连动杆3031和隔挡球3032一直处于承载管301的内部,因此,为了保证连动杆3031和隔挡球3032的使用寿命以及不引入新的杂质,可选地,连动杆3031和隔挡球3032的材料为耐高温的高密度氮化硅材料。For the above example, in some specific implementation manners, optionally, the material of the linkage rod 3031 and the barrier ball 3032 is high-density silicon nitride. It can be understood that during the heating and melting process of the silicon nitride B3 to be melted, the linkage rod 3031 and the blocking ball 3032 are always inside the carrying tube 301. Therefore, in order to ensure the use of the linkage rod 3031 and the blocking ball 3032 life and without introducing new impurities, optionally, the material of the linkage rod 3031 and the barrier ball 3032 is a high-density silicon nitride material with high temperature resistance.

对于上述示例,在一些具体的实施方式中,可选地,所述隔挡球3032的直径大于所述开口3011的直径。可以理解地,在本申请的具体实施过程中,为了防止待熔化的氮化硅B3从开口3011处掉落,因此,隔挡球3032的直径大于开口3011的直径,以保证当隔挡球3032下降与承载管301的底部贴合时能够完全遮挡住开口3011,即使当待熔化的氮化硅B3为颗粒状时,颗粒状的氮化硅B3也不会从开口3011处掉落。For the above example, in some specific implementation manners, optionally, the diameter of the barrier ball 3032 is larger than the diameter of the opening 3011 . It can be understood that, in the specific implementation process of the present application, in order to prevent the silicon nitride B3 to be melted from falling from the opening 3011, therefore, the diameter of the blocking ball 3032 is larger than the diameter of the opening 3011, so as to ensure that the blocking ball 3032 The opening 3011 can be completely covered when it is lowered to fit the bottom of the carrying tube 301 , even when the silicon nitride B3 to be melted is granular, the granular silicon nitride B3 will not fall from the opening 3011 .

对于上述示例,在一些具体的实施方式中,所述连动杆3031与所述升降机构304固定连接。可以理解地,为了便于隔挡球3032的上升或下降,在本申请的具体实施方式中,将连动杆3031与升降机构304固定地连接在一起,以实现通过升降机构304控制隔挡球3032的上升或下降,进而控制开口3011的遮挡或打开。For the above example, in some specific implementation manners, the linkage rod 3031 is fixedly connected with the lifting mechanism 304 . It can be understood that, in order to facilitate the rising or falling of the barrier ball 3032, in the specific embodiment of the present application, the linkage rod 3031 is fixedly connected with the lifting mechanism 304, so as to realize the control of the barrier ball 3032 through the lifting mechanism 304 rise or fall, and then control the blocking or opening of the opening 3011.

参见图5,本申请实施例还提供了一种氮掺杂剂加料方法,所述氮掺杂剂加料方法能够应用于前述的氮掺杂剂加料装置30中,所述氮掺杂剂加料方法包括:Referring to FIG. 5, the embodiment of the present application also provides a nitrogen dopant feeding method, which can be applied to the aforementioned nitrogen dopant feeding device 30, and the nitrogen dopant feeding method include:

S501、将多晶硅原料B1及硼掺杂剂B2放置于石英坩埚QC中并升温至1450℃以使得所述多晶硅原料B1及所述硼掺杂剂B2熔化形成含硼原子的硅熔体M';S501, placing the polysilicon raw material B1 and the boron dopant B2 in the quartz crucible QC and raising the temperature to 1450° C. to melt the polysilicon raw material B1 and the boron dopant B2 to form a silicon melt M′ containing boron atoms;

S502、将设定质量的待熔化的氮化硅B3投入至氮掺杂剂加料装置30中,并通过加热装置302升温至1800℃以使得所述待熔化的氮化硅B3熔化形成氮化硅熔体M";S502. Put the silicon nitride B3 to be melted with a set mass into the nitrogen dopant feeding device 30, and raise the temperature to 1800° C. through the heating device 302 so that the silicon nitride B3 to be melted is melted to form silicon nitride Melt M";

S503、通过升降机构304提升隔挡装置303,以使得所述氮化硅熔体M"通过承载管底部的开口滴落至所述含硼原子的硅熔体M'中。S503, using the lifting mechanism 304 to lift the blocking device 303, so that the silicon nitride melt M" drops into the boron atom-containing silicon melt M' through the opening at the bottom of the supporting tube.

可以理解地,当氮化硅熔体M"全部滴落至含硼原子的硅熔体M'后,待石英坩埚QC中的含氮原子和硼原子的硅熔体稳定后便可以开始拉制单晶硅 棒。It can be understood that when the silicon nitride melt M" is completely dropped into the silicon melt M' containing boron atoms, the drawing can be started after the silicon melt containing nitrogen atoms and boron atoms in the quartz crucible QC is stable. Monocrystalline silicon rods.

参见图6,本申请实施例还提供了一种氮掺杂单晶硅棒的制造系统50,所述制造系统50具体包括:根据前述所述的氮掺杂剂加料装置30,以及拉晶设备40;其中,Referring to Fig. 6, the embodiment of the present application also provides a nitrogen-doped single crystal silicon rod manufacturing system 50, the manufacturing system 50 specifically includes: the nitrogen dopant feeding device 30 according to the foregoing, and crystal pulling equipment 40; of which,

所述氮掺杂剂加料装置30用于将氮化硅熔体M"掺入所述拉晶设备40中石英坩埚QC内的含硼原子的硅熔体M'中;The nitrogen dopant feeding device 30 is used to mix the silicon nitride melt M" into the silicon melt M' containing boron atoms in the quartz crucible QC in the crystal pulling device 40;

所述拉晶设备40用于利用含氮原子和硼原子的硅熔体采用Czochralski法拉制单晶硅棒。The crystal pulling device 40 is used to pull single crystal silicon rods by Czochralski method using silicon melt containing nitrogen atoms and boron atoms.

需要说明的是,上述的拉晶设备1可以是拉晶炉中的比如导流筒、单晶硅棒提拉装置等与用于拉制单晶硅棒相关联的部件,以及比如石英坩埚QC、石墨加热器等与用于将多晶硅原料B1和硼掺杂剂B2熔化相关联的部件构成的设备,因此本申请中的氮掺杂剂加料装置30以及拉晶设备1可以在同一常规的拉晶炉中实现。It should be noted that the above-mentioned crystal pulling equipment 1 can be components associated with pulling single crystal silicon rods such as a draft tube and a single crystal silicon rod pulling device in a crystal pulling furnace, and such as a quartz crucible QC , graphite heater, etc. are used to melt the polysilicon raw material B1 and the boron dopant B2, so the nitrogen dopant feeding device 30 and the crystal pulling device 1 in the present application can be used in the same conventional pull Realized in the crystal furnace.

需要说明的是:本申请实施例所记载的技术方案之间,在不冲突的情况下,可以任意组合。It should be noted that: the technical solutions described in the embodiments of the present application may be combined arbitrarily if there is no conflict.

以上所述,仅为本申请的具体实施方式,但本申请的保护范围并不局限于此,任何熟悉本技术领域的技术人员在本申请揭露的技术范围内,可轻易想到变化或替换,都应涵盖在本申请的保护范围之内。因此,本申请的保护范围应以所述权利要求的保护范围为准。The above is only a specific implementation of the application, but the scope of protection of the application is not limited thereto. Anyone familiar with the technical field can easily think of changes or substitutions within the technical scope disclosed in the application. Should be covered within the protection scope of this application. Therefore, the protection scope of the present application should be determined by the protection scope of the claims.

Claims (9)

一种氮掺杂剂加料装置,所述氮掺杂剂加料装置设置于石英坩埚的正上方,所述氮掺杂剂加料装置包括:A nitrogen dopant feeding device, the nitrogen dopant feeding device is arranged directly above the quartz crucible, and the nitrogen dopant feeding device comprises: 底部设置有开口的承载管,所述承载管用于承载待熔化的氮化硅;A carrying tube with an opening at the bottom, the carrying tube is used to carry the silicon nitride to be melted; 环绕于所述承载管外侧的加热装置,所述加热装置用于加热所述待熔化的氮化硅使其完全熔化成氮化硅熔体;a heating device surrounding the outside of the carrying tube, the heating device is used to heat the silicon nitride to be melted to completely melt it into a silicon nitride melt; 设置于所述承载管内部的隔挡装置,所述隔挡装置能够与所述承载管的底部贴合以遮挡所述开口,以防止所述待熔化的氮化硅从所述开口处掉落至所述石英坩埚中;以及,所述隔挡装置能够与所述承载管的底部产生间隙以打开所述开口,以使得所述氮化硅熔体从所述开口处滴落至承载有含硼原子的硅熔体的所述石英坩埚中;A blocking device arranged inside the carrying tube, the blocking device can be attached to the bottom of the carrying tube to cover the opening, so as to prevent the silicon nitride to be melted from falling from the opening into the quartz crucible; and, the barrier device can create a gap with the bottom of the carrier tube to open the opening, so that the silicon nitride melt drips from the opening to the carrier containing silicon melt of boron atoms in said quartz crucible; 升降机构,所述升降机构用于提升或下降所述隔挡装置。A lifting mechanism, the lifting mechanism is used to lift or lower the blocking device. 根据权利要求1所述的氮掺杂剂加料装置,其中,所述承载管的材料为高密度氮化硅。The nitrogen dopant feeding device according to claim 1, wherein the material of the carrying tube is high-density silicon nitride. 根据权利要求1所述的氮掺杂剂加料装置,其中,所述加热装置为电阻式加热器。The nitrogen dopant feeding device according to claim 1, wherein the heating device is a resistance heater. 根据权利要求1所述的氮掺杂剂加料装置,其中,所述隔挡装置包括连动杆和隔挡球;其中,所述连动杆和所述隔挡球固定连接。The nitrogen dopant feeding device according to claim 1, wherein the barrier device comprises a linkage rod and a barrier ball; wherein the linkage rod and the barrier ball are fixedly connected. 根据权利要求4所述的氮掺杂剂加料装置,其中,所述连动杆和所述隔挡球的材料为高密度氮化硅。The nitrogen dopant feeding device according to claim 4, wherein the material of the connecting rod and the blocking ball is high-density silicon nitride. 根据权利要求5所述的氮掺杂剂加料装置,其中,所述隔挡球的直径大于所述开口的直径。The nitrogen dopant feeding device according to claim 5, wherein the diameter of the barrier ball is larger than the diameter of the opening. 根据权利要求5所述的氮掺杂剂加料装置,其中,所述连动杆与所述升降机构固定连接。The nitrogen dopant feeding device according to claim 5, wherein the linkage rod is fixedly connected with the lifting mechanism. 一种氮掺杂剂加料方法,所述氮掺杂剂加料方法能够应用于权利要求1至7任一项所述的氮掺杂剂加料装置中,所述氮掺杂剂加料方法包括:A nitrogen dopant feeding method, the nitrogen dopant feeding method can be applied to the nitrogen dopant feeding device according to any one of claims 1 to 7, the nitrogen dopant feeding method comprising: 将多晶硅原料及硼掺杂剂放置于石英坩埚中并升温至1450℃以使得所述多晶硅原料及所述硼掺杂剂熔化形成含硼原子的硅熔体;placing the polysilicon raw material and the boron dopant in a quartz crucible and raising the temperature to 1450° C. to melt the polysilicon raw material and the boron dopant to form a silicon melt containing boron atoms; 将设定质量的待熔化的氮化硅投入至氮掺杂剂加料装置中,并通过加热装置升温至1800℃以使得所述待熔化的氮化硅熔化形成氮化硅熔体;Putting a set mass of silicon nitride to be melted into the nitrogen dopant feeding device, and raising the temperature to 1800° C. through a heating device so that the silicon nitride to be melted is melted to form a silicon nitride melt; 通过升降机构提升隔挡装置,以使得所述氮化硅熔体通过承载管底部的开口滴落至所述含硼原子的硅熔体中。The barrier device is lifted by the lifting mechanism, so that the silicon nitride melt drops into the silicon melt containing boron atoms through the opening at the bottom of the supporting tube. 一种氮掺杂单晶硅棒的制造系统,所述制造系统包括:根据权利要求1至7任一项所述的氮掺杂剂加料装置,以及拉晶设备;其中,A manufacturing system for nitrogen-doped single crystal silicon rods, the manufacturing system comprising: the nitrogen dopant feeding device according to any one of claims 1 to 7, and crystal pulling equipment; wherein, 所述氮掺杂剂加料装置用于将氮化硅熔体掺入所述拉晶设备中石英坩埚内的含硼原子的硅熔体中;The nitrogen dopant feeding device is used to mix the silicon nitride melt into the silicon melt containing boron atoms in the quartz crucible in the crystal pulling equipment; 所述拉晶设备用于利用含氮原子和硼原子的硅熔体采用直拉法拉制单晶硅棒。The crystal pulling equipment is used for pulling single crystal silicon rods by Czochralski method using silicon melt containing nitrogen atoms and boron atoms.
PCT/CN2022/122591 2021-09-29 2022-09-29 Nitrogen dopant feeding apparatus and method, and system for manufacturing nitrogen-doped monocrystalline silicon rod Ceased WO2023051693A1 (en)