WO1997012410A1 - Electrical energy devices using conductive ceramic fibers - Google Patents

Electrical energy devices using conductive ceramic fibers Download PDF

Info

Publication number
WO1997012410A1
WO1997012410A1 PCT/US1996/015621 US9615621W WO9712410A1 WO 1997012410 A1 WO1997012410 A1 WO 1997012410A1 US 9615621 W US9615621 W US 9615621W WO 9712410 A1 WO9712410 A1 WO 9712410A1
Authority
WO
WIPO (PCT)
Prior art keywords
conductive ceramic
fibers
battery
batteries
metal
Prior art date
Application number
PCT/US1996/015621
Other languages
French (fr)
Inventor
David James
Daniel B. Ii Allison
John J. Kelley
James B. Doe
Original Assignee
Energetics Systems Corporation
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Energetics Systems Corporation filed Critical Energetics Systems Corporation
Priority to DE69632594T priority Critical patent/DE69632594T2/en
Priority to EP96933950A priority patent/EP0868757B1/en
Priority to AT96933950T priority patent/ATE268058T1/en
Priority to BR9610751-0A priority patent/BR9610751A/en
Priority to JP9513739A priority patent/JPH11512869A/en
Priority to AU72486/96A priority patent/AU702715B2/en
Publication of WO1997012410A1 publication Critical patent/WO1997012410A1/en

Abstract

The performance of electrochemical energy devices such as batteries, fuel cells, capacitors and sensors is enhanced by the incorporation of ceramic materials in the form of fibers, powder, chips and substrates. Preferred are fibers having a length varying from about 10 to about 10,000 microns. The fibers may also be coated with metal.

Description

Electrical Energy Devices Using Conductive Ceramic Fibers
Priority is claimed to provisional application 60/004553, filed September 29, 1995.
TECHNICAL FIELD The present invention relates to electrochemical devices such as batteries, fuel cells, capacitors and sensors which employ electrically conductive ceramic materials, fibers, powder, chips and substrates therein to improve the performance of the electrochemical device.
BACKGROUND ART
Tnere are numerous applications which involve the transfer of electrical current m environments wnich are highly corrosive or otherwise degrading to metallic conductors. Most notably are electrochemical devices operating under highly corrosive conditions and high temperatures. Examples of such applications are the use of electrodes for the chlor-al ali cell to make chlorine gas, electrodes for metal recovery, electrodes m hydrogen/oxygen fuel cells, electrodes for producing ozone, electrolysis of water and electrodes m high temperature solid oxide fuel cells. Most of these applications involve tne contact of an electroαe with an electrolyte under conditions wnich render the electrode ineffective during prolonged use. Tne loss of effectiveness can be gradual, such loss being manifested by reduced current-carrying capacity of the electrode. Exemplary types of conditions which render electrodes ineffective as they are used m current-carrying applications are described below.
One such condition involves chemical attack of the electrode by corrosive gas which is evolved from the electrolyte as it is decomposed during use. For example, the evolution of chlorine gas, a highly corrosive material, from an aqueous chloride-containing electrolyte such as, in the chlor-alkali cell is exemplary.
Another type of condition involves passivation of the electrode as it combines with the anions from the electrolyte to form an insoluble layer on its surface. This passivation condition occurs when the product from the electrochemical reaction can not diffuse from the electrode surface and this produces a blocking of the electrochemical sites and/or pores. The end result is a diminishing of the electrode current carrying capacity. An example of this passivation is the lead dioxide electrode in an aqueous sulfuric acid solution. Another type of condition which renders electrodes ineffective involves the dissolution of the electrode by the electrolyte. The use of a zinc electrode in an aqueous potassium hydroxide solution is exemplary. Various types of batteries such as secondary (rechargeable) batteries: lead-acid (Pb/Pb02) , NaS, Ni/Cd, NiMH (metal hydride), Ni/Zn, Zn/AgO, Zn/Mn02, Zn/Br2; and primary (non-rechargeable) batteries: Zn/Mn02, AgCl/Mg, Zn/HgO, Al/Air(02), Zn/Air(02), Li/S02, Li/Ag2CrO„ and Li/Mn02 exist. Although a variety of batteries are available, the lead- acid battery remains favored for uses such as starting internal combustion engines, electric vehicle motive power, as well as portable and emergency power for industrial and military applications. Lead-acid batteries include a cathode comprising a lead alloy grid (active material support structure and electrical network structure contact with the battery terminals) having PbO, active material thereon; and an anode comprising sponge lead on a grid. The active material on a grid is called the plate and electrically, the anode (Pb) plate is negative and the cathode (Pb02) plate is positive. A separator, either glass fibers or porous plastic, is used to separate the cathode and anode from direct contact when the plates are in sulfuric acid electrolyte. For the lead-acid battery, the rated capacity (ampere-hours) depends on the total amount of electrochemicaUy active material in the battery plates, the concentration and amount of sulfuric acid electrolyte, the discharge rate and the percent utilization (conversion of active material into ampere-hours) for the active materials (the cathode or Pb02 usually being the limiting factor) .
During discharge of a lead-acid battery, the lead and lead dioxide active materials are converted to lead sulfate. The lead sulfate can form an undesirable, insulating layer or passivation around the cathode active material particles which reduces the active material utilization during discharge. This passivatmg layer can be the result of improper battery charging, low temperature operation, and/or excessive (high current) discharge rates. In order to increase the cathode active material utilization, which is desirable for battery performance, means to increase the cathode active material porosity which increases the amount of active material contact with the sulfuric acid and/or active material conductivity which minimizes resistance and electrical isolation of the active material particles are useful. However, raising the cathode active material porosity tends to increase the tendency for a loosening and possible loss of active material from the plate as well as electrical isolation of the active material from the grid structure. Wrapping the cathode plate with a glass mat holds the loosened active material tightly to the plate and minimizes the tendency for active material sediment (electrochemicaUy lost cathode material) in the bottom of the battery container. The addition of conductive materials (carbon, petroleum coke, graphite) to increase the conductivity of the cathode active material is well-known, but these materials are degraded rapidly from the oxygen generated at the cathode during charging.
Since the lead-acid battery anode is very conductive, the additives for the sponge lead active material have concentrated on improving low temperature battery performance and cycle life. The fundamental additive to the anode is the expander which is comprised of lampblack, barium sulfate and lignosulfonic acid mixed with the lead oxide (PbO) carrier agent. The expander addition to the sponge lead inhibits densification or decrease in the sponge lead porosity. If the anode active material becomes too dense, it is unable to operate at low temperatures and can no longer sustain practical current discharges.
In the manufacture of lead-acid batteries, cathode electrodes are usually prepared from lead alloy grids which are filled with an active paste that contains sulfated lead oxide. This sulfated lead oxide is then later converted or formed into sponge lead for the anode and lead dioxide for the cathode. In an alternative construction, known as tubular cathode plates, the cathode active material is a sulfated lead oxide powder that is poured into a non-conductive tube (braided or woven glass or polyethylene) containing a protruding lead alloy rod or spine. Several of these tubes make up the grid structure and electrical connections are made to the terminals by the protruding lead alloy rods. The tubular cathodes and the usual plate anodes are then assembled into elements and these are then placed in a battery container. The cells are filled with electrolyte and the battery is subjected to the formation process. See details on lead-acid batteries, by Doe in Kirk-Othmer: Encyclopedia of Chemical Technology, Volume 3 (1978), page 640-663.
During lead-acid battery formation, active material particles in contact with the grid are formed first and particles further away from the grid are formed later. This tends to reduce the efficiency of formation. An apparent solution to this problem is addition of a conductive material to the active material paste. The additive should be electrochemicaUy stable in the lead-acid system both with respect to oxidation and reduction at the potentials experienced during charge and discharge of the cell, as well as to chemical attack by the sulfuric acid solution. The use of barium metaplumbate and other ceramic perovskite powder and plating additives to the lead-acid battery anode and cathode are reported to enhance the formation of lead-acid batteries. See U. S. Patent No. 5,045,170 by Bullock and Kao. However, these additives are limited to the lead-acid battery system and require up to a 50 weight percent addition to be effective.
For other battery systems, the cathode materials such as, Mo03, V205, Ag2Cr04 and (CFx)n that are used in primary lithium batteries are typically mixed with carbon, metal or graphite powder to improve the overall cathode electrical conductivity and therefore, the utilization of the cathode material. Depending on the battery design, the current collector is either the cathode material itself or a nickel screen pressed into the cathode material. The current collector for the anode (lithium) is a nickel screen pressed into the lithium metal. The separator between the lithium battery cathode and anode is typically a non-woven polypropylene, Teflon or polyvinyl chloride membrane. The electrolyte for the lithium battery is an organic solvent such as propylene carbonate, dimethyl sulphoxide, dimethylformamide, tetrahydrofuran to which some inorganic salt such as, LICIO4, LiCl, LiBr, LiAsF6 has been added to improve the solution ionic conductivity. Hughes, Ha pson and Karunathilaka (J. Power Sources, 12 (1984), pages 83-144)) discuss the enhancement techniques used for improving the cathode electrical conductivity for lithium anode cells. While the addition of the materials to improve the cathode conductivity and utilization are feasible, the amount of additive material required means that much less electrochemical active cathode material that will be available, and in some lithium battery designs, because of volume limitations, that can be critical.
Other battery systems requiring that the cathode have improved conductivity and thereby, improved cathode (NiOOH/Ni (OH) 2) active material utilization are secondary nickel batteries such as, Ni/Cd, Ni/Zn and Ni/MH (metal hydride) . The electrolyte for the nickel battery system is usually potassium hydroxide solution and the separator between the anode and cathode is non-woven polypropylene. To enhance the cathode conductivity, graphite is added but this material is not long lasting as it is gradually oxidized to carbon dioxide. In addition to the degradation of the graphite, there is a gradual build-up of carbonate ions which reduces the conductivity of the electrolyte. See discussion on nickel batteries in "Maintenance-Free Batteries" by Berndt.
A sodium-sulfur battery comprises molten sulfur or molten sodium polysulfide as a cathode, molten sodium as an anode, and a non-porous solid electrolyte made of beta alumina that permits only sodium ions to pass. The sulfur or sodium polysulfide m the cathode has an inferior electrical conductivity m itself. The art has attempted to address this problem by adding conductive fibers such as metal fiber or carbon fiber to the molten sulfur or molten sodium polysulfide. For general information, see U.S. Patent Numbers 3, 932,195 and 4,649,022. These types of fibers however, are prone to corrosion in the electrochemical environment of a sodium-sulfur battery. A need therefore continues for sodium- sulfur batteries which employ chemically stable conductive ceramic materials therein. Another type of electrical energy generating device, as is known m the art, is the fuel cell such as acid fuel cells, molten carbonate fuel cells, solid polymer electrolyte fuel cells and solid oxide fuel cells. A fuel cell is an apparatus for continually producing electric current by electrochemical reaction of a fuel with an oxidizing agent.
More specifically, a fuel cell is a galvanic energy conversion device that chemically converts a fuel such as hydrogen or a hydrocarbon and an oxidant that catalytically react at electrodes to produce a DC electrical output. In one type of fuel cell, the cathode material defines passageways for the oxidant and the anode material defines passageways for fuel. An electrolyte separates the cathode material from the anode material. The fuel and oxidant, typically as gases, are continuously passed through the cell passageways for reaction. The essential difference between a fuel cell and a battery is that there is a continuous supply of fuel and oxidant from outside the fuel cell. Fuel cells produce voltage outputs that are less than ideal and decrease with increasing load (current density) . Such decreased output is in part due to the ohmic losses within the fuel cell, including electronic impedances through the electrodes, contacts and current collectors. A need therefore exists for fuel cells which have reduced ohmic losses. The graphite current collectors used in phosphoric acid and solid polymer electrolyte fuel cells, to the cathode metal oxides such as, praseodymium oxide, indium oxide used in solid oxide fuel cells and to the nickel oxide cathode used in molten carbonate fuel cells are examples of a need for conductive additives. See generally, "Handbook of Batteries and Fuel Cells", Edited by Linden. Multilayer surface mount ceramic chip capacitors which store electrical energy are used extensively by the electronics industry on circuit boards. A typical multilayer surface mount chip capacitor is comprised of alternating multilayers of dielectric (ceramics such as BaTi03) electrodes (metals such as Pd or Pd-Ag) . The end caps or terminations of the capacitor are typically a metallic (Ag/Pd) in combination with a conductive glass. This termination is the means of contact to the internal electrodes of the multilayer ceramic capacitor. The development of other electrodes such as nickel and copper to reduce costs and the use of low cost conductive additives to the glass are actively being sought. See generally, Sheppard (American Ceramic Society Bulletin, Vol. 72, pages 45-57, 1993) and Selcuker and Johnson (American Ceramic Society Bulletin, 72, pages 88-93, 1993) . An ultra-capacitor, sometimes referred to as a super capacitor, is a hybrid encompassing performance elements of both capacitors and batteries. Various types of ultra¬ capacitors are shown in "Ultracapacitors, Friendly Competitors and Helpmates for Batteries," A.F. Burke, Idaho National Engineer Laboratory, February 1994. A problem associated with an ultracapacitor is high cost of manufacture.
Sensors, as are known in the art, generate an electrical potential in response to a stimulus. For example, gas sensors such as oxygen sensors generate an electrical potential due to interaction of oxygen with material of the sensor. An example of an oxygen sensor is that described by Taka i (Ceramic Bulletin, 67, pages 1956-1960, 1988) . In this design, the sensor material, titania (Ti02) , is coated on an alumina (A1203) substrate with individual lead connections for the substrate and the titania components. The development of higher electrical conductive titania to improve the oxygen sensor response is an on-going process. Another sensor, humidity, is based upon the electrical conductivity of MgCr204- Ti02 porous ceramics is discussed by Nitta et al . (J. American Ceramic Society, 63, pages 295-300, 1980) . For humidity sensing, leads are placed on both sides of the porous ceramic plaque and the sensor is then placed in the air-moisture stream for resistivity (inverse of electrical conductivity) measurements. The relative humidity value is then related to the measured resistivity value. With this design, the porous ceramic resistivity value, as low as possible, is critical because of the need for a rapid measurement response time (seconds) that can be related to an accurate relative humidity value. Another type of electrical device, as is known in the art, is a bipolar battery. Such a battery typically comprises an electrode pair constructed such that cathode and anode active materials are disposed on opposite sides of an electrically conductive plate, that is, a bipolar plate. The cells that have this electrode pair are configured such that the cell-to-cell discharge path is comparatively shorter and dispersed over a large cross-sectional area, thus providing lower ohmic resistance and improved power capabilities compared to unipolar batteries such as automobile batteries. The bipolar electrodes are stacked into a multicell battery such that the electrolyte and separators lie between adjacent bipolar plates. The Lead-acid batteries are attractive candidates for bipolar construction because of the high power capabilities, known chemistry, excellent thermal characteristics, safe operation and widespread use. However, such lead-acid batteries with bipolar construction often fail due to the corrosion of the electrically conductive plate when in contact with the active material. A need therefore exists for bipolar batteries which have improved corrosion resistance, low resistivity and reduced weight. For general information on bipolar batteries, see Bullock (J. Electrochemical Society, 142, pages 1726-1731, 1995 and U. S. Patent No. 5,045,170) and U. S. Patent No. 4,353,969.
Although the devices of the prior art are capable of generating and storing electrical energy, and acting as oxygen and relative humidity sensors, there is a need for improved materials of construction for reasons of diminished corrosion, higher capacity and/or higher electrical conductivity which overcome the disadvantages of the prior art. In addition to the previously mentioned materials used in the above applications, there are several U. S. Patents which delineate the electrochemical use of electrically conductive ceramics such as the sub-oxides of titanium which are formed from the reduction of titanium dioxide in hydrogen or carbon monoxide reducing gases at high temperatures (1000°C or greater) . For example, U. S. Patent No. 5,126,218 discusses the use of TiOx (where x=1.55 to 1.95) as a support structure (grids, walls, conductive-pin separators) , as a conductive paint on battery electrodes and as powder in a plate for the lead-acid battery. A similar discussion occurs in U. S. Patent No. 4,422,917 which teaches that an electrochemical cell electrode is best made from bulk material where the TiOx has its x vary from 1.67 to 1.85, 1.7 to 1.8, 1.67 to 1.8, and 1.67 to 1.9. The said mentioned electrode materials are suitable for electrocatalytically active surfaces when it includes material from the platinum group metals, platinum group metal alloys, platinum group metal oxides, lead and lead dioxide. The electrodes are also suitable for metal plating, electrowinning, cathodic protection, bipolar electrodes for chlorine cells, tile construction, and electrochemical synthesis of inorganic and organic compounds.
Oxides of titanium are discussed in U. S. Patent No. 5,173,215 which teaches that the ideal shapes for the Magneli phases
Figure imgf000012_0001
where n is 4 or greater) are particles that have a diameter of about one micron (1 micron (denoted μ) is 10'6 meter (denoted m) ) or more and a surface area of 0.2 m2/g or less.
The U. S. Patent No. 5,281,496 delineates the use of the Magneli phase compounds) in powder form for use in electrochemical cells. The use of powder is intended for the electrode structure only.
U. S. Patent No. 4,931,213 discusses a powder containing the conductive Magneli phase sub-oxides of titanium and a metal such as copper, nickel, platinum, chromium, tantalum, zinc, magnesium, ruthenium, iridium, niobium or vanadium or a mixture of two of more of these metals.
DISCLOSURE OF THE INVENTION The invention is directed to solving the problems of the prior art by improving electrochemical devices such as batteries, fuel cells, capacitors, sensors and other electrochemical devices as follows: (1) In batteries for example, there will be an improved discharge rate, increased electrochemicaUy active material utilization, improved charging efficiency, reduced electrical energy during the formation of electrochemicaUy active materials and decreased electrical resistance of the electrochemicaUy active material matrix; (2) In fuel cells, for example, there will be decreased electrical resistance of the current collectors and cathode materials as well as increased electrical chemical efficiency of the reactants; (3) In capacitors, for example, there will be development of less expensive electrodes and conductive glass; (4) In sensors, there will be the development of lower resistive titanium dioxide for oxygen sensors and lower resistive binary compounds containing titanium dioxide for relative humidity sensors; and (5) In other electrochemical devices, for example, there will be the development of more corrosion resistant and current efficient electrodes for electrolysis, electrosynthesis.
As used herein, conductive ceramic materials include conductive ceramic compositions such as solids, plaques, sheets (solid and porous) , fibers, powders, chips and substrates (grids, electrodes, current collectors, separators, foam, honeycomb, complex shapes for use in components such as grids made by known methods such as weaving, knitting, braiding, felting, forming into paper-like materials, extrusion, tape casting or slip casting) made from conductive ceramic compositions having metal containing additives and metallic coatings thereon, or made from non-conductive ceramic compositions having metal containing additives and metallic coatings dispersed thereon.
The electrically conductive ceramic materials for use in the invention, when in the form of fibers, powders, chips or substrate, are inert, light weight, have high surface area per unit weight, have suitable electrical conductivity, as well as high corrosion resistance. Typically, the electrically conductive ceramic fibers, powders, chips or substrate herein have an electrical conductivity of 0.1 (ohm-cm)"1 or more. Electrically conductive ceramic fibers, powder, chips or substrate useful in the invention include an electrically conductive or non-electrically conductive ceramic matrix, preferably with a metal containing additive and/or metallic coating. Ceramic matrix materials which may be employed include, the oxides of the metals titanium, and vanadium and the oxides of zirconium, and aluminum. The reduced oxides of titanium and vanadium have a certain amount of intrinsic electrical conductivity and the oxides of zirconium and aluminum are intrinsically insulators. All mentioned ceramic oxides have different chemical and physical attributes and these materials cover a wide range of applicability. Either ceramic metal oxide can have the electrical conductivity increased by the addition or plating or coating or deposition of singly or a mixture thereof of metallic d-block transition elements (Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Y, Zr, Nb, Mo, Tc, Ru, Rh, Pd, Ag, Cd, La, Hf, Ta, W, Re, Os, Ir, Pt, Au) , Lanthanides (Ce, Pr, Nd, P , Sm, Eu, Gd, Tb, Dy, Ho, Tm, Yb, Lu) and/or by the addition or plating or coating or deposition singly or a mixture thereof of selected main-group elements (B, Al, Ga, In, Tl, Si, Ge, Sn, Pb, As, Sb, Bi, Se,
Te) and/or the oxides, halides, carbides, nitrides and borides of the aforementioned elements. Chemical reduction processes for the selected mixtures reduce the ceramic to its final electrically conductivity form. Similarly, chemical oxidation processes may be used to form superstoichiometric titanium oxide in which the atomic oxygen to titanium ratio is slightly above 2.
The electrically conductive ceramic materials, fibers, powders, and chips mentioned in this invention can be used to enhance the electrical conductivity and thereby, the utilization of the electrochemicaUy active materials in cathode for the following primary and secondary battery systems: lithium batteries, zinc air batteries, aluminum air batteries, alkaline batteries, Leclanche batteries, nickel batteries, lead-acid batteries, and sodium-sulfur. The electrically conductive ceramic substrate as mentioned in this invention would be suitable for fuel cell electrodes and current collectors and bipolar plate batteries. In addition, the electrically conductive ceramic materials, fibers, powders, chips and substrate according to this invention would be suitable for oxygen and humidity sensors as well as multilayer chip capacitors and ultracapacitors. The electrode made from this invention can also be useful as an anode or cathode, whichever is applicable, in electrochemical devices including batteries and in an electrolytic cell generating ozone, chlorine gas, or sodium, recovering metals from wastewater and purification of metals by electrolysis.
The electrically conductive ceramic materials, fibers, powders, chips and/or substrates therein may impart superior battery discharge and charging performance, battery cycle life, battery charge retention, battery weight reduction, deep battery discharge recovery, as well as battery structure vibration and shock resistance. Batteries such as lead-acid batteries which employ electrically conductive ceramic materials, fiber, powder, chips and/or substrates therein advantageously may require reduced electrical energy during formation. Fuel cells utilizing electrically conductive ceramic materials, fibers, powder and/or substrate for the current collector and the electrodes may have longer operating life because of superior corrosion resistance and enhanced performance because of superior electrical conductivity. The use of electrically conductive ceramic materials, fibers, powder, chips and substrates from this invention may impart low cost manufacturing, superior electrical resistivity performance in oxygen and humidity sensors, multilayer chip capacitors, and ultracapacitors.
Other advantages of the present invention will become apparent as a fuller understanding of the invention is gained from the detailed description to follow. MODES FOR CARRYING OUT THE INVENTION In accordance with the invention, electrically conductive ceramic materials, fibers, powders, chips and substrates are either added to components or used to construct components for electrochemical devices such as batteries, fuel cells, capacitors, sensors, and other electrochemical devices. The type of conductive ceramic material used depends on the type of chemical, electropotential and electrochemical environments to which the conductive ceramic materials will be subjected.
Preferred Ceramic Materials The preferred starting materials for electrically conductive sub-oxide titanium ceramics according to this invention are the following: Ti02 (preferably rutile) , Ti, Ti203, Ti305,, metal (chromium, copper, nickel, platinum, tantalum, zinc, magnesium, ruthenium, iridium, niobium, and vanadium or a mixture of two or more of the aforementioned metals) -containing intercalated graphite, graphite and carbon. Also possible, the addition of singly or a mixture thereof metallic d-block transition elements (Sc, Ti, V, Cr, Mn, Fe,
Co, Ni, Cu, Zn, Y, Zr, Nb, Mo, Tc, Ru, Rh, Pd, Ag, Cd, La, Hf, Ta, W, Re, Os, Ir, Pt, Au) , Lanthanides (Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Tm, Yb, Lu) and by the addition singly or a mixture thereof selected main-group elements (B, Al, In, Tl, Si, Ge, Sn, Pb, As, Sb, Bi, Se, Te) and/or the oxides, halides, carbides, nitrides and borides of the aforementioned elements. All materials used should have a purity level that excludes deleterious substances for this process as well as the projected use. The preferred starting materials for electrically conductive sub-oxide vanadium ceramics according to this invention are the following: V205, V203, V02, V, metal (chromium, copper, nickel, platinum, tantalum, zinc, magnesium, ruthenium, iridium, niobium, and vanadium or a mixture of two or more of the aforementioned metals) - containing intercalated graphite, graphite, and carbon. Also possible, the addition of singly or a mixture thereof metallic d-block transition elements (Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Y, Zr, Nb, Mo, Tc, Ru, Rh, Pd, Ag, Cd, La, Hf, Ta, W, Re, Os, Ir, Pt, Au) , Lanthanides (Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Tm, Yb, Lu) and by the addition singly or a mixture thereof selected main-group elements (B, Al, In, Tl, Si, Ge, Sn, Pb, As, Sb, Bi, Se, Te) and/or the oxides, halides, carbides, nitrides and borides of the aforementioned elements. All materials used should have a purity level that excludes deleterious substances for this process as well as the projected use.
The teachings of U. S. Patent No. 4,422,917 state that the conductive materials of choice for the sub-oxides of titanium should consistent essentially of Ti407 and Ti509 in order to maximize the conductivity. This concept was further extended by the teachings of U. S. Patent No. 5,173,215 which stated that it is more proper to speak of the appropriate conductive sub-oxides of titanium as Magneli phases with the general formula Tin02n-1 where n=4 or greater. TiO is never considered in either patent as an important component because of reported instability and less than desirable resistance to chemical attack. For the sub-oxides of titanium, Ti407 has been measured with a conductivity value of 1585 (ohm-cm)"1, Ti50Q has been measured with an electrical conductivity value of 553 (ohm-cm)"1, and the electrical conductivity of TiO has been measured to be 3060 (ohm-cm)"1. This TiO value is almost twice that of the Magneli phase Ti407. With this invention, the TiO is considered to be an important component of the over-all electrical conductivity. Through judicious selection of the sub-oxide titanium reduction process conditions to make a well-defined TiO structure and with the aforementioned metal compound additions to the starting materials for the titanium oxides, a synergism effect occurs during processing and results in a stable and chemical resistance TiO structure within the ceramic matrix of the sub-oxides of titanium. Separately, the '917 and '215 patents do not teach super- oxides of titanium (superstoichiometric "Ti02") in which the atomic oxygen to titanium ratio is slightly above 2. A preferred composition of matter for the electrically conductive ceramic material, fibers, powders, chips and substrates of the sub-oxides of titanium with additives is as follows:
Constituent Weight Percent (%) Tin02n.: where n=4 or greater 80-90
TiO 0-10
Ti203 and Ti305 >>>1
M oxides, and/or borides, and/or carbides, 0-10 and/or nitrides and/or free metal, wherein the sum of the above percentages is less than or equal to 100% and wherein M= Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Y, Zr, Nb, Mo, Tc, Ru, Rh, Pd, Ag, Cd, La, Hf, Ta, W, Re, Os, Ir, Pt, Au, Ce, Pr, Nd, Pm, S , Eu, Gd, Tb, Dy, Ho, Tm, Yb, Lu, B, Al, Tl, Si, Ge, Sn, Pb, As, Sb, Bi, Se, Te.
Another composition of matter for the electrically conductive ceramic material, fibers, powders, chips and substrates of the sub-oxides of titanium, if there were no metal compound additives, and if the starting materials were only TiO, (preferably rutile) and metal-containing intercalated graphite, is:
Constituent Weight Percent (%)
Tin02n_1 where n=4 or greater 90-100
M oxides and/or free metal Where M= Cr, Cu, Ni, Pt, Ta, Zn, Mg, Ru,
Ir, Nb, V. 0-10
A preferred composition of matter for the electrically conductive ceramic material, fibers, powders, chips and substrates of the sub-oxides of vanadium with additives is as follows:
Constituent Weight Percent (%)
VOX (x=l to 2.5) 50-90
M oxides, and/or borides, and/or carbides, and/or nitrides and/or free metal 10-50 wherein the sum of the above-noted weight percents is less than or equal to 100 and wherein M= Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Y, Zr, Nb, Mo, Tc, Ru, Rh, Pd, Ag, Cd, La, Hf, Ta, W, Re, Os, Ir, Pt, Au, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Tm, Yb, Lu, b, Al, Tl, Si, Ge, Sn, Pb, As, Sb, Bi, Se, Te.
Another composition of matter for the electrically conductive ceramic material, fibers, powders, chips, and substrates of the sub-oxides of vanadium, if there were no metal compound additives, and if the starting materials were only V203 and metal-containing intercalated graphite, is: Constituent Weight Percent (%)
VOX (x = 1 to 2.5) 90-100
M oxides and/or free metal Where M= Cr, Cu, Ni, Pt, Ta, Zn, Mg, Ru,
Ir, Nb, V either singly or mixtures thereof. 0-10
For electrically conductive ceramics made by plating, coatings, and deposition of metals and/or conductive ceramic, the composition of matters are as follows:
Constituent Weight Percent (%)
A1203 85-90
M oxides and/or free metal 5-15 Where M= Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Y, Zr, Nb, Mo, Tc, Ru, Rh, Pd, Ag, Cd, La, Hf, Ta, W, Re, Os, Ir, Pt, Au, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Tm, Yb, Lu, In, Tl, Sn, Pb, Sb, Bi, Se, Te either singly or mixtures thereof. Constituent Weight Percent (%)
Zr02 85-95
M oxides and/or free metal 5-15
Where M= Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Y, Zr, Nb, Mo,
Tc, Ru, Rh, Pd, Ag, Cd, La, Hf, Ta, W, Re, Os, Ir, Pt, Au, Ce,
Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Tm, Yb, Lu, B, Al, Tl, Si,
Ge, Sn, Pb, As, Sb, Bi, Se, Te singly or mixtures thereof.
Constituent Weight Percent (%)
A1203 40-48 Zr02 40-48
M oxides and/or free metal 4-20 Where M= Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Y, Zr, Nb, Mo, Tc, Ru, Rh, Pd, Ag, Cd, La, Hf, Ta, W, Re, Os, Ir, Pt, Au, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Tm, Yb, Lu, B, Al, Tl, Si, Ge, Sn, Pb, As, Sb, Bi, Se, Te, singly or mixtures thereof.
Examples of applications in which the conductive ceramic materials of the present invention can be used are the following: (1) the use of fibers, powder, or chips in the cathode active materials of the lead-acid, lithium, nickel, Zn, and metal air batteries; (2) the use of fibers, powder or chips to make substrates for use as current collectors and electrodes and the use of fiber, powder, and chips in electrodes for fuel cells; (3) the use of fibers, powders or chips to make substrates for use as electrodes for electrosynthesis, cathodic protection, electrocatalysis, electrolysis, and metal recovery; (4) the use of fibers, powder and chips to make substrates which can act as bipolar electrode construction for lead-acid batteries; (5) the use fibers, powders and chips to make substrates for use as electrodes and the use of fibers and powder in glass for capacitors; (6) the use of fibers, powders, chips to make a substrate which can act as an electrode in sensors. If so desired, the electrodes fabricated from this invention can be plated, coated, or deposited with metals to enhance their electrochemical properties.
Forming of Shaped Materials Electrically conductive ceramic materials and fibers can be formed from the oxides of titanium or vanadium material that may or may not have metal containing additives and "in situ" reduction agents dispersed therein. Shaping may be done on either electrically-conducting or electrically non¬ conducting materials. In the latter case, activation of the oxide to a conducting state is done on the shaped material. For titanium or vanadium materials, this activation may be done by chemical reduction. Normally non-conducting oxides such as A1203 or Zr02 are made conducting by plating of conducting materials, as is discussed below. In the following, various possible shapes are discussed.
Fibers
These ceramic matrixes are made into fibers by known fiber-making processes such as the viscous suspension spinning process (Cass, Ceramic Bulletin, Vol. 70, pages 424-429, 1991) with and without metal-containing intercalated graphite, or by the sol-gel process (Klein, Sol-Gel Technology for Thin Films, Fibers, Preforms, Electronics, and Speciality Shapes, Noyes Publications, pages 154-161) , and or by either the slurry or solution extrusion process (Schwartz,Handbook of Structural Ceramics, page 4.55, 1992) . The procedures for sample slurry or slip preparation, drawing or extruding material as well as the appropriate drying to remove water, heating to burn off organics, and sintering are discussed in detail in these articles. After the sintering operation at 1000-2000DC, these ceramic fiber materials are made electrically conductive through reduction in a furnace at 1000-2000°C whose atmosphere is either hydrogen, carbon monoxide or mixtures of these gases. In addition, depending on the metal containing additives in the starting ceramic matrix, "in situ" reduction and/or decomposition processes occur during the drying, heating, sintering and reduction cycles via the use of "in situ" reduction materials such as carbon, metal-containing intercalated graphite, graphite, and metal powders incorporated either singly or mixtures thereof into the ceramic matrix. Once after the reduction process has ended, the fibers are cooled in a dry atmosphere and stored until use. At this point, the electrically conductive ceramic fibers are now ready for use. All initial starting materials are in powdery form and the ceramic matrix powders have been mixed to obtain a homogeneous mixture of materials before preparing the slurry or slip prior to the fiber making process. For enhanced ceramic matrix reactivity, it is preferred that the particle size of the powders be in the range of 40 to 150 microns. Preferably, the electrically conductive ceramic fibers have an aspect ratio of greater than 1 and an electrical conductivity value of 0.1 (ohm-cm)"1 or greater.
Non-electrically conductive ceramic fibers are formed from alumina (A1203) or zirconia (Zr02) or zirconia-alumina material with no metal containing additives or "in situ" reduction agents. These ceramic matrixes are then made into fibers by the previously mentioned viscous suspension spinning process, or by the sol-gel process, and/or by either the slurry or solution process. The sample slurry or slip preparation, drawing or extruding material as well as the appropriate drying to remove water, heating to burn off organics, sintering and storage conditions are the same as discussed for the electrically conductive ceramics matrixes. All the initial starting materials are in powdered form and are mixed to obtain a homogeneous mixture before slurry or slip preparation prior to the fiber-making process. It is preferred that the particle size of the starting powders be in the range of 40 to 150 microns. The ceramic fibers so obtained are considered to be insulators or non-electrically conductive.
Details of Spinning and Sintering to Make Fibers
In forming the conductive ceramic fibers by solution spinning and sintering, a suspension of particles of ceramic material in a solution of destructible carrier dissolved in a solvent is prepared. The fibers then are wet or dry spun from the suspension, dryed and fired to drive off the carrier and sinter the fiber. Preferably, the particle size is 5 microns or less, and polyvinyl alcohol/ water system may be used as a carrier/solvent.
After the aforementioned components have been mixed at a certain compositional ratio characteristic of the desired ceramic material, the resulting mixture is dispersed or dissolved in a polymer compound solution. Thus, a spinning solution is obtained. Optionally, the aforementioned mixture may be roasted at an elevated temperature such as 900-1, 100°C for about 1-5 hours before it is dispersed or dissolved in the polymer compound-containing solution. Examples of polymer compounds which may be used in the present invention include polyacrylonitrile, polyethylene, polypropylene, polyamide, polyester, polyvinyl alcohol polymers ("PVA"), cellulose derivatives (e.g., methyl cellulose, hydroxyethyl cellulose, hydroxyethylmethyl cellulose, etc.), polyvinylpyrrolidone, polyacrylamide, polyethylene glycol, etc.
Generally, the degree of saponification of the aforementioned PVA polymer may be 70-100 mol%, more preferably 85-100 moll, most preferably 95-100 mol%. The degree of polymerization of the polymer may be 500-20,000, preferably 1,000-15,000.
Polyvinyl alcohol polymers which may be employed include ordinary unmodified polyvinyl alcohol as well as modified polyvinyl alcohols can also be used. As modified polyvinyl alcohols, a saponified copolymer of vinyl acetate and a copolymerizable comonomer may be used. Examples of these comonomers include vinyl esters such as vinyl propionate, vinyl stearate, vinyl benzoate, vinyl saturated branched fatty acid salts, etc., unsaturated monocarboxylic acids such as acrylic acid, methacrylic acid, crontonic acid, etc. and their alkyl esters, unsaturated polycarboxylic acids such as maleic acid, maleic anhydride, fumaric acid, itaconic acid, etc. and their partial esters or total esters, acrylonitrile, methacrylonitrile, acryiamide, methacrylamide, olefinsulfonic acids such as ethylenesulfonic acid, allylsulfonic acid, methacrylsulfonic acid, etc. and their salts, α-olefins such as ethylene, propylene, butene, α-octene, α-dodecene, α- octadecene, etc., vinyl ether, silane-containing monomers, etc. The concentrations of the aforementioned comonomers with respect to the copolymer may be less than 20 mol%.
As other modified polyvinyl alcohols, products obtained by modifying a vinyl acetate homopolymer or the aforementioned saponified copolymer can be used. Examples of modifying reactions include acetylation, urethanation, phosphoric acid esterification, sulfuric acid esterification, sulfonic acid esterification, etc.
A useful spinning solution for forming fibers for use in the present invention may be obtained by dispersing or dissolving a ceramic material or a substance which can be converted to a conductive ceramic material by heat treatment (preferably a fiber) in the aforementioned polymer compound solution.
As the solvents of the polymer compound solution, water or other solvents which can solubilize polymer compounds may be used.
Examples of solvents other than water include alcohols, ketones, ethers, aromatic compounds, amides, amines, sulfones, etc. These solvents may be mixed with water at certain ratios. Polyvinyl alcohol polymers may be employed as the polymer compound. The solvents such as water, dimethyl sulfoxide, glycerin, ethylene glycol, diethylene glycol, N- met ylpyrrolidone, dimethylformamide, and their mixtures can be advantageously used. In the present invention, dry spinning may be employed to produce fibers for use in the claimed invention. As is known in the art, dry spinning entails spinning a solution drawn into air or another gas from a die or in a die-free state. The spinning draft typically is about 0.1-2.0. Subsequently, the resulting precursor fiber is heat-treated. The precursor fiber may be stretched before heat treatment. In a typical heat treatment, the fiber is baked for several minutes to several hours in a desired atmosphere to achieve a desired level of conductivity in the fiber. Then, the fiber is cooled.
There are no special restrictions on the diameter of the conductive fiber obtained. Typically, the diameter is about 200 um or less, preferably 100 μm or less, more preferably 50 μm or less, most preferably 20 μm or less. There are no special restrictions on the lower limit.
In the aforementioned spinning solution, the weight ratio of the polymer compound with respect to the conductive ceramic material or substance which can be converted to conductive ceramic material by heat treatment is about 15 wt% or less and 3 wt% or more, preferably 10 wt% or less and 3 wt% or more, respectively.
When the aforementioned spinning solution is prepared, a dispersant for the conductive ceramic material or substance which can be converted to conductive ceramic material by heat treatment can also be used. Examples of dispersants include anionic emulsifiers, nonionic emulsifiers, and cationic emulsifiers such as polyoxyethylene (10) octylphenyl ether and sodium dodecylsulfate. Moreover, polyacrylic acid and its salts, polystyrene, neutralized maleic anhydride copolymers, maleic anhydride-isobutene copolymer, and other polymer dispersion stabilizers may be used.
There are no special restrictions on the total solid content of the aforementioned spinning solution. Generally speaking, however, the solid content is about 20-70 wt%. After the spinning solution has been dry-spun, it is dried. Thus, a continuous precursor fiber is obtained.
Sintering of mixtures of ceramic powders, optionally with metals, may also be employed to manufacture conductive ceramic fibers. In the manufacture of conductive ceramic materials by sintering, ceramic matrix material and metal additive are combined with a binder, and subjected to elevated temperatures in a selected atmosphere. The specific temperatures and the atmosphere depend on the composition to be sintered. See for example, U.S.Patent 4,931,213 directed to sintering of substoichiometric Ti02 having Cu therein. Metal containing additives which may be incorporated into the ceramic matrix by sintering have a relatively high melting point and a low vapor pressure to minimize loss of the metal containing additive. Metals which may be included in ceramic matrices to provide conductive ceramic material for use in the invention include Cu, Ni, Co, Ag, Pt, Ta, Zn, Mg, Ru, Ir, Nb, V, Sn, SnO, Sn02, Pb, and alloys thereof, as well as other metals which are stable in the electrochemical system of the device. For example, conductive ceramic fibers formed of non- stoichiometric Ti02 such as Ti407 and/or Ti509 matrix having Cu therein may be employed.
Coating of fibers
The conductive ceramic fibers employed in the invention may be coated with a metal such as Cu, Ni, Co, Ag, Pt, Ta, Zn, Mg, Ru, Ir, Nb, V, W, Sn, SnO, Sn02, Pb, as well as alloys thereof. Choice of metal coating on the conductive ceramic materials and fibers depends on the active material, and/or the component in which the coated conductive ceramic fibers are employed. For example, in lead-acid batteries, especially useful metal coatings include Sn-Pb alloys wherein Sn may be up to 90%, remainder Pb in thicknesses of about 0.1-1.0 mil on a conductive ceramic fiber material of either Ti40 and/or Ti509. In alkaline batteries such as NiCd, NiMH, Ni-Fe, Ni-Zn and Mn02-Zn, especially useful metal coatings include Ni, Ag and Cu in thicknesses of about 0.1-1.0 mil on a conductive ceramic fiber matrix of substoichiometric TiO, such as Ti407 and/or Ti5Os intercalated with Cu. In Li batteries such as Li-Mn02, especially useful coatings include Ni, Ag, Cu, Li, and SnO, in thicknesses of about 0.1-1.0 mil on a conductive ceramic fiber matrix of substoichiometric TiO, such as Ti407 and/or TisO?.
In Ni batteries such as NiCd, and NiMH, especially useful metal coatings include Co, Ni, NiCo alloys on a ceramic matrix of Ti407 and/or Ti509, each of which optionally may have Cu therein. In sensors such as gas sensors, especially useful coatings include Sn02 on, for example, Ti407 and/or Ti5Og ceramic matrix, each of which may have Cu therein. In capacitors such as TiO, on Ti407 and/or Ti509, carbon or graphite on Ti407 and/or Ti509, especially useful coatings include Cu on a ceramic matrix of Ti407 and/or Ti50?.
The specific choice of conductive ceramic matrix material and metal containing additive therein, as well as the composition of metal coating thereon, may be determined by the art skilled in accordance with the specific electrochemical system of the device in which the fibers or other conductive ceramic materials are employed. The primary requirements are that the fiber or other conductive ceramic materials and metal coating be compatible with the electrochemistry of the battery. Accordingly, the choice of metal coating on the conductive ceramic fiber or material will vary depending on the electrochemistry of the device, the adherence of the metal coating to the ceramic matrix of the conductive ceramic fiber or material. Generally, the metal coating should not be attacked by the electrolyte in the device.
The thickness of the metal coating on the conductive ceramic fiber or other conductive ceramic materials similarly depends on the device in which the conductive ceramic fibers or other conductive ceramic materials are employed. Generally, the thickness of the applied metal coating should be sufficient to provide a pore free coating. For example, lead-acid batteries which employ conductive ceramic fibers formed of Ti407 and/or Ti50« having Sn0 therein may have about a .001 inch thick coating of Pb, Sn, or Sb thereon. Similarly, alkaline batteries such as NiCd which employ conductive ceramic fibers formed of a Ti4Oτ and/or Ti509 matrix having Ni, Co, Cn, or NiCo alloys therein may have a .001 inch thick coating of Ni thereon. In Li batteries such as LiMnO, which employ conductive ceramic fibers formed of a Ti407 and/or Ti509 matrix having Li, Ni or Mn therein may have about a .001 inch thick coating of Cu thereon. In Ni batteries which employ conductive ceramic fibers formed of a Ti40- and/or Ti509 matrix having Ni or Co therein may have about a .001 inch thick coating of Co thereon.
Well known methods such as chemical vapor deposition, plasma spraying, laser deposition, and solution dipping may be employed to apply a metal coating onto the conductive ceramic fibers or other conductive ceramic materials, provided that that method does not attack the underlying substrate. For example, tin, lead and alloys thereof can be applied by immersion dipping to provide a coating thickness on the order of microns to mils. In a further aspect of the invention, the conductive ceramic fibers or other conductive ceramic materials may be coated with alternating metal layers of differing compositions. Useful combinations of conductive ceramic fibers or other conductive ceramic materials having metal coatings thereon are shown in Table 1.
TABLE 1
Figure imgf000029_0001
Figure imgf000030_0001
Active pastes which employ conductive ceramic fibers or other conductive ceramic materials therein typically have about 0.1-30% of the active paste, preferably about 5-20%, as conductive ceramic fibers depending on the conductivity of the conductive ceramic fiber composition. In an active paste, the size of the fibers is sufficient to provide uniform distribution of the ceramic fiber material throughout the paste. Useful sizes of conductive ceramic fibers may vary from about 2-10 microns diameter.
Examples of components in which conductive ceramic fibers or other conductive ceramic materials may be employed include the grids of electrodes for batteries. The conductive ceramic fibers may be present in a grid in an amount of about 80 to 100 % by weight of the grid.
In capacitors such as double layer capacitors and ultracapacitors, materials and components which may employ conductive ceramic fibers or other conductive ceramic materials such as Ti407 and Ti509 wherein the fibers are present in amounts of about 30 to 100% based on the total weight of the plates of the capacitor.
In fuel cells, materials and components which may employ conductive ceramic fibers or other conductive ceramic materials and molded products such as electrodes formed of those fibers or other conductive ceramic materials include H: and O, electrodes.
In sensors such as 02 gas or organic vapor sensors, materials and components which may employ conductive ceramic fibers or other conductive ceramic materials include electrodes.
In bipolar batteries such as lead-acid bipolar batteries, materials and components which may employ conductive ceramic fibers or other conductive ceramic materials include for example, the active material. Conductive ceramic fibers or other conductive ceramic materials may be formed into complex shapes suitable for use in components such as grids by known methods such as weaving, knitting, braiding, extrusion, and slip casting. The conductive ceramic fibers or other conductive ceramic materials may be formed into porous paper-like materials by known methods. The choice of method depends on the porosity and strength desired in the grid. For example, a grid formed by felting of a liquid slurry of conductive ceramic fibers has a surface area greater than that obtainable by processes such as weaving.
When forming the components by extrusion, a blend of conductive ceramic precursor material and a binder is formed by mixing. The amounts of conductive ceramic precursor material and binder may vary within wide limits depending on the shape to be extruded as well as the specific ceramic material and binder compositions. Useful binder compositions include those commonly employed in the manufacture of extruded ceramic products. Examples of useful binders include organic binders such as polyethylene, polypropylene, stearates, celluloses such as hydroxy propyl cellulose, polyesters and the like. Typically, greater amounts of binder materials are employed when forming intricately shaped articles. The specific amounts and composition of binder for use with a specific conductive ceramic precursor material to provide a blend suitable for extrusion can readily be determined by those skilled in the art. The extruded product then is dried and fired to produce the desired component such as a plaque or a bipolar electrode.
In slip casting, as is generally known in the art, a slurry of a conductive ceramic precursor material and a liquid vehicle such as water, optionally with an organic binder and surfactants, is cast into a mold to provide the desired shaped article. The specific amounts of ceramic material, organic binder and liquid vehicle can be varied depending on the density desired in the cast product. The resulting cast product is dried and fired by conventional techniques known in the art.
Felting of conductive ceramic fibers or other conductive ceramic materials also may be employed to produce components such as grids for use in electrochemical devices such as batteries. Felting can be performed as shown in the John Badger patent directed to glass mat separators. Green fibers, as well as certain sintered fibers, of the ceramic materials may be employed in well known weaving processes to produce components such as grids which then are fired for use in electrochemical devices such as batteries.
Fiber requirements
The conductive ceramic fibers for use in the invention have a diameter and a length consistent with the processing requirements of the paste or other component in which the conductive ceramic fiber is to be employed. Generally, preferred fibers have lengths of 10 to 10,000 μ and length to diameter ratios of 1 to 100. Typically, when conductive ceramic fibers are employed in active pastes, the fibers are about 0.125 inches (3,175 μ) to 0.250 inches (6,350 μ) long and about 0.002 to 0.007 inches diameter. The fibers, moreover, should be capable of withstanding substantial levels of shear stress. The fibers are mixed into the active material paste by conventional mixers.
The grid for use in an electrode of a device such as a battery or fuel cell may include varying amounts of ceramic fibers or other conductive device depending on the type of device. For example, in a lead acid battery, the current collector may be formed of about fifty percent, up to one hundred percent of conductive ceramic fiber material such as Ti407 or Ti509 having therein an oxide which is conductive, stable to sulfuric acid and capable of nucleating PbO,. Such oxides include Sn02, W03, (TiO and Ti40, and/or Ti509) . Similarly, in alkaline batteries such as NiCd, about 0.1 - 20 % conductive ceramic fibers of (TiO and (Ti407) and/or Ti407) having Ni therein may be employed.
When the ceramic fibers are formed into a grid by deposition of the fibers from a liquid slurry, the diameter of the fibers may be about 0.002-0.007 inches and have a length of about 0.125 to about 0.250 inches. Generally, the conductive ceramic fibers should be long enough to yield intersecting joints and/or span the width of the mesh size of a grid to yield a conductive pathway. Specific fiber diameters and lengths can therefore be determined by the art skilled for a specific application for a given fiber composition.
Conductive ceramic fibers may be mixed with active materials such as PbO or PbS04 to provide improved active material pastes. The conductive ceramic fibers are uniformly distributed throughout the active material paste to provide low resistance paths for flow of electrons between the active material particles and the grid. These low resistance paths may function to reduce the internal resistance of the device in which the active material is employed, especially at low states of charge.
Conductive ceramic fibers or other conductive ceramic materials may be employed in various devices such as batteries, fuel cells, capacitors, and sensors. Batteries may be classified according to the shape of the electrodes. These classifications include paste type electrodes and tubular electrodes. Paste type electrodes have a grid of lead or lead alloy, or a grid formed of woven, knitted, or braided conductive ceramic fibers. Tubular electrodes are made by inserting a cylindrical tube of braided fibers such as glass fibers and polyester fibers around a grid, and then filling the tube with active material. Tubular type electrodes typically are employed as positive electrodes, whereas paste type electrodes are typically positive or negative electrodes. In accordance with the invention, it is contemplated that conductive ceramic fibers or other conductive ceramic materials may be employed in paste and tubular electrodes.
The conductive ceramic fibers or other conductive ceramic materials may be admixed with additional fibers and the resulting blend employed in the active paste and current collector of a battery. The amount of additional fiber in the paste or current collector may vary depending on the physical properties desired. Useful blends are contemplated to include Ti407 and/or TiB09 having Sn02, Cu, Ni, Co, and the like therein with any of carbon fibers, nickel fibers, stainless steel fibers, olefin fibers such as polyethylene, polypropylene, cellulosic fiber, polyesters such as Dacron, and composite fibers such as lead-coated glass fibers. The amount of additional fibers may vary from about 1 to 30 % based on the total weight of active material. These additional fibers may be employed to impart additional mechanical strength and corrosion resistance to components formed of the conductive ceramic fibers. Examples of useful blends are given in Table II. TABLED
Ceramic
1 Example Conductive Metal Olefm
No. Fiber % Fiber % Fiber %
1 Ti,07' Ni 60-20% Polypropylene 30-70% 10%
2 TiA1 Stainless Polypropylene 30-70% Steel 60-70% 10-20%
3 Sn02 90% - Polypropylene 10%
4 Ti407 - Polypropylene 90% 10%
5 Ti407 - Polyester 50-90% 10-50%
1 Ti407 intercalated with Cu therein.
2 Ti509 intercalated with Nb therein.
The conductive ceramic fibers or other conductive ceramic materials employed in the invention typically have conductivity sufficient to provide an increase in conductivity of the active material but yet are sufficiently porous and provide enhanced electrochemical utilization of the active material. The active material paste to which the conductive ceramic fibers are added may influence the amount of conductive ceramic fibers employed therein. For instance, in a lead-acid battery where the active paste material of the cathode is Pb02 having about 5-10% conductive ceramic fiber of Ti407, and/or Ti509 matrix, having about 0.5-1.8% metal containing Sn02 therein may be used in the cathode. In alkaline batteries such as Zn-MnO, wherein the less conductive Mn02 material is used as the active paste material, about 1 - 30% conductive ceramic fiber of matrix of Ti407 and/or Ti509 having Cu therein may be employed in the active material. In lithium containing batteries such as Li-Mn02, about 1 - 10 % conductive ceramic fiber or other conductive ceramic materials of matrix Tι40, and/or Tι50Q having Cu therein may be employed. In nickel containing batteries such as NiMH, about 1 - 10 % conductive ceramic fiber of matrix Tι407 and/or Tιs09 havmg Co therein may be employed. Typically, conductive ceramic fibers may be used as the additive m the active material in amounts of about 0.1% to 40% by weight of active material.
The diameter and length of the conductive ceramic fiber for use devices such as batteries, fuel cells, sensors, and capacitors may vary according to the material and component to be formed therefrom, as well as the conductivity desired m the component or paste material in which the fiber is to be employed. The method used to make the specific material or component in which the conductive ceramic fiber is employed is also a factor in determining the diameter and length of the conductive ceramic fiber. In formmg an active paste which mcludes conductive ceramic fibers, the fibers should have dimensions sufficient to be processable with the active material of the paste. Typically, the size of the conductive ceramic fibers may vary from about 0.125-0.250 inches long and a diameter of about 0.001-0.005 mches, i.e. dimensions sufficient to retain the fibrous form with the active paste material.
Various batteries may be improved by using conductive ceramic fibers. For example, NiCd batteries, the Ni foam electrode may be pasted with an active material of Nι(0H)2 having about 10 % conductive ceramic fibers of Tι407 and/or Tι509 having Ni therein. In NiMH batteries, a conductive ceramic fiber of Tι40 and/or Tι50α having Ni or Cu therein can be added to both the cathode of NiOH and anode formed of mischmetal hydride. In NiZn batteries, a conductive ceramic fiber of Tι407 and/or Tι509 having Cu therein may be added to a paste of ZnO.
Nickel electrodes also may employ conductive ceramic fibers by adding the fibers to the electrode material, principally NiOOH. In a nickel-cadmium alkaline cell, porous nickel plates are used in both the positive and negative electrodes. The active material for the positive and negative electrodes is contained within the nickel plates. The positive plate contains nickel hydroxide while the negative plate contains cadmium hydroxide. To form improved electrodes for use in a Ni-Cd cell, a blend of NiOH, CdOH and 0.5-5% of conductive ceramic fiber of Ti407 and/or Ti509, each having Cu, Ni therein, is mixed with about 0.5-5% organic polymeric binder such as carboxy methylcellulose in aqueous solution sufficient to provide an active material paste.
In lithium containing batteries such as Li-AgV,05, Li-CF, Li-CuO, Li-FeS, Li-FeS2, Li-I2, Li-Mn02, Li-MoS2, Li-V205, Li-SOCl2, and Li-S02, especially useful ceramic conductive fibers include Li, Co, Cu or Ni in a ceramic matrix of Ti407 and/or Ti509. Ceramic conductive fibers or other conductive ceramic materials such as Ti407 or Ti409 having Co or Cu therein can be manufactured using the viscous suspension spinning process described by Cass in Ceramic Bulletin, No. 70, pages 424-429, 1991 or by other processes described herein. In batteries in which a lithium compound of lithium thermodynamic activity less than that of lithium metal is the anode material (one example of which is lithium intercalated into graphite or petroleum coke, see J. M. Tarascon and D. Guyo ard, Electrochimica Acta, 38: 1221-1231 (1992) ) and the cathode material is selected from the group containing AgV205, CFX, CuO, Mn02, FeS, FeS2, TiS2, MoS2, V205, S0C12, S02, and I2, and lithium-containing materials derived therefrom (including those cathode materials suitable for "rocking chair" batteries as described by Michel Armand in "Materials for Advanced Batteries", eds. D. W. Murphy, J. Broadhead, and B. C. H.
Steele, Plenum Press, New York, at page 160 and as described by J. M. Tarascon and D. Guyomard, Electrochimica Acta 38: 1221-1231 (1992) ) , ceramic conductive fibers may be added to the cathode material to enhance current collection. Especially useful ceramic conductive fibers include Ni, Co, Cu and NiCo alloy in a ceramic matrix of Ti407 and/or TiB09 with or without TiO. Ceramic conductive fibers such as Ti407-Ni, Ti509-Cu are available from ACI.
While the present invention has been described with respect to various specific embodiments and examples it is to be understood that the invention is not limited thereto and that it can be variously practiced within the scope of the following claims.
Powders Electrically conductive ceramic powders are formed from the oxides of titanium or vanadium material that may or may not have metal containing additives and "in situ" reduction agents such as carbon, metal-containing intercalated graphite, graphite, and metal powders incorporated singly or mixtures dispersed therein. All materials for making electrically conductive ceramic powders are in powdery form and mixed to obtain a homogeneous mixture. For enhanced ceramic matrix reactivity, it is preferred that the particle size of the powders be in the range of 40 to 150 microns. This powder mixture is placed in a furnace at 300°C to burn off the organics and then heated up to 1000-2000°C in a reducing atmosphere of hydrogen or carbon monoxide or mixtures of these gases. In general, the reduced powdered mixture needs to be ground up to meet the particle size requires for an aspect ratio of 1.
Chips Electrically conductive chips are made from the oxides of titanium or vanadium material that may or may not have metal containing additives and "in situ" reduction agents such as carbon, metal-containing graphite, graphite, and metal powders incorporated singly or mixtures dispersed therein. All materials for making electrically conductive ceramic chips are in powdery form and mixed to obtain a homogeneous mixture. A slip is made from this mixture and used in a tape casting process (See Mistier, Tape Casting Chapter in Engineered Materials Handbook, Vol. 4, 1992) which makes a dried or "green" (unfired) tape of the ceramic matrix. This dried tape is then cut into ceramic chips with a pasta or like cutting machine. The chips are then placed in a furnace in air at 300°C to burn off the organics, then the furnace temperature is raised to 1000-2000°C for sintering and after this the furnace atmosphere, but not the temperature, is changed to a reducing gas such as hydrogen or carbon monoxide or a mixture of both gases. For some electrochemical device applications, the dried tape can be thermally processed and reduced without cutting into chips for use as electrodes or layers in a multilayer chip capacitor. After thermally processing and reducing, the chips are roughly rectangular in size and the aspect ratio (aerodynamic definition (long dimension/short dimension) ) is 8 or less. The hot chips are cooled in a dry, inert atmosphere and stored in a sealed container. At this point, the electrically conductive ceramic chips are ready to use.
Non-electrically conductive ceramic chips are made from alumina (A1203) or zirconia (Zr02) or zirconia-alumina material with no metal-containing additives or "in situ" reduction agents. All materials for making non-electrically conductive ceramic chips are in powdered form and are mixed to obtain a homogeneous mixture. A slip is made from this mixture and used in tape casting to make a dried tape of the ceramic matrix. This dried tape is then cut into ceramic chips with a pasta or like cutting machine. The chips are then placed in a furnace in air at 300°C to burn off the organics, then the furnace temperature is raised to 1000-2000°C for sintering and after this the furnace atmosphere, but not the temperature, is changed to a reducing gas such as hydrogen or carbon monoxide or a mixture of both gases. For some electrochemical device applications, the dried tape can be thermally processed without cutting into chips. The dried tape can then be cut into electrodes and coated with a metal or metals, for a particular application. After thermally processing, the chips are roughly rectangular in size and the aspect ratio (aerodynamic definition (long dimension/short dimension)) is 8 or less. The hot chips are cooled in a dry, inert atmosphere and stored in sealed containers. At this point, the non- electrically conductive ceramic chips are ready to be coated, plated, or deposited with a metal or metals to make them electrically conductive and/or catalytically active.
Substrates For substrate (grids, electrodes, current collectors, separators, porous sheets, foam, honey-comb sheets, solid sheets) fabrication, the electrically conductive ceramic materials, fibers, powders and chips can be mixed with a suitable binding agent and filler and the resulting mixture molded in a ram press or extruded into the desired shape. The shape is then vitrified in a non-oxidizing atmosphere at 1000- 2000°C to inhibit the oxidation of the sub-oxides of the titanium or vanadium. After this vitrification process, the cooled substrates are ready for use. The ceramic foam can be made by the Scotfoam process (Selee Corporation) .
Activation of non-electrically conducting materials Since the electrically conducting ceramic fibers, powders, chips and substrates have their own intrinsic electrical conductivity developed by metal compound additives and/or by a reduction of the metal sub-oxide, it only remains for the non-electrically conducting ceramic fibers, powders, chips and substrates to be made electrically conductive. The increase in electrical conductivity for the non-electrically conductive ceramic materials as well as electrically conductive substrates is done by plating or coating or deposition of singly or a mixture thereof metallic d-block transition elements (Sc,Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Y, Zr, Nb, Mo, Tc, Ru, Rh, Pd, Ag, Cd, La, Hf, Ta, W, Re, Os, Ir, Pt, Au, Lanthanides (Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Tm, Yb, Lu) and by the addition or plating or coating or deposition singly or a mixture thereof selected main-group elements (In, Tl, Sn, Pb, Sb, Bi, Se, Te) . All materials used should have a purity level that excludes deleterious substances for this process as well as the projected use.
There are several metal plating, metal deposition and ceramic coating techniques that can be used to treat the non-electrically conductive material and they are as follows: (1) electroless plating for non-conductors using a reducing solution of either formaldehyde or hydrazine to plate out the desired metal or metals (see Lowenheim, Electroplating, pages 387-425, 1978 and 1994 Products Finishing Directory, page 112- 130) ; (2) thermal metal spraying (See Thorp, Chemical Engineering Progress, pages 54-57, 1991) of the desired metal or metals and electrically conductive ceramic; and (3) layer- by-layer deposition:ion beam sputtering and laser deposition (Beardsley, Scientific American, pages 32-33, 1995 and Wasa, et al., Science and Technology of Thin Film Superconductors-2, pages 1-2) to deposit electrically conductive ceramic materials as defined in this invention, and any other method to provide suitable plating, coating or deposition of the desired metal. Once the non-electrically conductive ceramics have been interacted with metal, metals or electrically conductive ceramic, they are now ready for use.

Claims

1. An electrical energy device having at least one component having conductive ceramic fibers therein, said fibers having a length of about 10 to about 10,000 μ (1 μ = IO"6 ) and a length to diameter ratio of about 1 to about 20.
2. The device of claim 1 wherein said conductive ceramic fibers have a ceramic matrix and metal containing additive dispersed within said ceramic matrix.
3. The device of claim 2 wherein said device is capable of at least one of either generating electrical energy or storing electrical energy.
4. The device of claim 3 wherein said device is at least one of batteries, fuel cells, capacitors, and sensors
5. The device of claim 4 wherein said device is a battery.
6. The device of claim 5 wherein said battery is at least one of lead-acid batteries, alkaline batteries, sulfur containing batteries, lithium containing batteries, and nickel containing batteries.
7. The device of claim 2 wherein said conductive ceramic fibers have at least one metal coating thereon.
8. The device of claim 7 wherein said metal coating is substantially the same composition as said metal containing additive in said fibers.
9. The device of claim 6 wherein said battery is a lead acid battery.
10. The device of claim 6 wherein said battery is an alkaline battery.
11. The device of claim 10 wherein said alkaline battery is any of Zn-Ag02, Zn-AgO, Zn-AgN02, Zn-Ag2Pb02, Zn-HgO, Zn- Mn02.
12. The device of claim 11 wherein said alkaline battery includes at least one conductive ceramic fiber selected from the group of titanium suboxides and titanium superoxides.
13. The device of claim 6 wherein said sulfur containing battery is a sodium-sulfur battery.
14. The device of claim 13 wherein said sodium-sulfur battery includes at least one conductive ceramic fiber comprising TiO and an oxide selected from the group of Ti407, Ti509, copper-intercalated Ti407 and copper-intercalated Ti509.
15. The device of claim 6 wherein said device is a lithium containing battery of any of Li-AgV205, Li-CF, Li-CuO, Li-FeS, Li-FeS2, Li-I, Li-Mn02, Li-MoS2, Li-V,05, Li-TiS2, Li- S0C12, Li-SO,.
16. The device of claim 15 wherein said lithium containing battery includes at least one conductive ceramic fiber selected from the group of substoichiometric titanium and superstoichiometric titanium dioxide.
17. The device of claim 6 wherein said device is a Ni containing battery of any one of Ni-Cd, Ni-H2, Ni-Zn, Ni-MH and Ni-Fe.
18. The Ni containing battery of claim 17 wherein said battery includes at least one conductive ceramic fiber selected from the group of Ti407 intercalated with Cu, and Ti509 intercalated with Cu.
19. The device of claim 3 wherein said device is a fuel cell.
20. The device of claim 3 wherein said device includes at least one electrode having conductive ceramic fibers therein, said electrode having at least one of a current collector and active material.
21. The device of claim 20 wherein said conductive ceramic fibers are present in at least one of said current collector or said material.
22. The device of claim 19 wherein said fibers are present in said collector in an amount of about 50 to 100 % by weight of said collector.
23. The device of claim 20 wherein said fibers are present in said paste in an amount of about to % by weight of said paste.
24. The device of claim 21 wherein said matrix material is selected from the group of oxides, carbides, nitrides, and borides.
25. The device of claim 24 wherein said oxide is selected from the group of substoichiometric titanium dioxides, superstoichiometric titanium dioxides, and perovskite oxides.
26. The device of claim 25 wherein said perovskite oxide is tungsten oxide.
27. The device of claim 24 wherein said metal containing additive is selected from the group of Cu, Ni, Co, Ag, Pt, Ta, Zn, Mg, Ru, Ir, Nb, V, Sn, SnO, Sn02, Pb, Pd, Ir and alloys thereof.
28. The device of claim 27 wherein said oxide is substoichiometric titanium dioxides and said metal containing additive is selected from the group of Sn, SnO, and Sn02.
29. The device of claim 3 wherein said device is in the form of a capacitor.
30. The device of claim 29 wherein said capacitor includes conductive ceramic fiber therein.
31. The device of claim 30 wherein said conductive ceramic fibers are selected from the group of titanium suboxide and titanium superoxides.
32. The device of claim 3 wherein said sensors include at least one of thermal sensors and chemical sensors.
33. The device of claim 32 wherein said thermal sensor is in the form of single fibers or bundles of conductive, doped ceramic fibers.
34. The device of claim 33 wherein said chemical sensor is in the form of a sheet, paper, nonwoven or woven mat, and composed principally of conductive ceramic fibers.
35. A lead-acid battery having a plurality of electrodes therein, said electrode comprising an active material composition and a current collector, wherein conductive ceramic fibers are included in at least one said active material and said current collector.
36. The lead acid battery of claim 35 wherein said active material composition is lead dioxide and said conductive ceramic fibers have a substoichiometric titanium dioxide matrix and a Sn-Pb alloy dispersed throughout said matrix.
37. The lead acid battery of claim 36 wherein said current collector comprises conductive ceramic fibers from the group of substoichiometric titanium and superstoichiometric titanium.
38. The lead acid battery of claim 37 wherein said conductive ceramic fiber is a ceramic matrix of substoichiometric titanium dioxide having Sn-Pb alloy therein.
39. The lead acid battery of claim 38 wherein said substoichiometric titanium dioxide is Ti407.
40. The device of claim 5 wherein the anode compartment comprises a lithium material of thermodynamic activity less than that of lithium metal.
41. The device of claim 40 wherein the cathode compartment comprises a material containing manganese.
42. The device of claim 40 wherein the electrolyte material comprises an organic polymer.
43. The device of claim 40 wherein the anode compartment comprises a carbon material selected from the group containing graphite and petroleum coke.
44. The device of claim 5 wherein the battery is of bipolar design.
45. A battery which comprises an electrically conducting ceramic comprising an electrically conducting vanadium oxide.
46. A battery which comprises an electrically conducting ceramic comprising an oxide selected from the group of Al203 and Zr02 coated with a metal.
PCT/US1996/015621 1995-09-29 1996-09-27 Electrical energy devices using conductive ceramic fibers WO1997012410A1 (en)