JPS63293802A - Laminated magnetic thin film and magnetic head using the same - Google Patents
Laminated magnetic thin film and magnetic head using the sameInfo
- Publication number
- JPS63293802A JPS63293802A JP12811287A JP12811287A JPS63293802A JP S63293802 A JPS63293802 A JP S63293802A JP 12811287 A JP12811287 A JP 12811287A JP 12811287 A JP12811287 A JP 12811287A JP S63293802 A JPS63293802 A JP S63293802A
- Authority
- JP
- Japan
- Prior art keywords
- thin film
- magnetic
- laminated
- film
- magnetostriction constant
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Pending
Abstract
Description
【発明の詳細な説明】
〔産業上の利用分野〕
本発明は、低磁歪定数、高飽和磁束密度、高透磁率を有
する積層磁性薄膜に関し、特に磁気ディスク装a、VT
Rなどに用いる磁気ヘッドおよび磁気ヘッドのコア材料
に適した積層磁性薄膜に関する。Detailed Description of the Invention [Field of Industrial Application] The present invention relates to a laminated magnetic thin film having a low magnetostriction constant, high saturation magnetic flux density, and high magnetic permeability, and particularly for magnetic disk devices a, VT
The present invention relates to a laminated magnetic thin film suitable for a magnetic head used for magnetic heads and the like and a core material of the magnetic head.
磁気ヘッド材料はヘッドの記録時の磁気飽和を防ぐため
に高飽和磁束密度を有することが必要である。またヘッ
ドの記録再生効率の面から低保磁力、高透磁率の特性を
有することが必要であり、そのためには磁歪定数が零に
近いことが好ましい。The magnetic head material needs to have a high saturation magnetic flux density to prevent magnetic saturation during recording of the head. Further, from the viewpoint of recording and reproducing efficiency of the head, it is necessary to have characteristics of low coercive force and high magnetic permeability, and for this purpose, it is preferable that the magnetostriction constant is close to zero.
従来、高飽和磁束密度を有するFeの磁歪定数を零とす
るために、例えば、アール・エム・ボゾルス(R,M、
Bozorth)による1951年発行のフエロマグ
ネテイズム(Ferromagnetism) 676
〜680ページに論じられているとおり、Feに他の元
素を添加することが行なわれてきた。Conventionally, in order to make the magnetostriction constant of Fe, which has a high saturation magnetic flux density, zero, for example, R.M. Bosols (R, M,
Ferromagnetism 676, published by Bozorth in 1951.
Additions of other elements to Fe have been made, as discussed on pages 680-680.
しかし、上記従来技術のようにFeに他の元素を添加す
ることにより磁歪定数の調整を行うと、多くの場合、飽
和磁束密度が低下してしまうという問題があった。However, when the magnetostriction constant is adjusted by adding other elements to Fe as in the prior art described above, there is a problem in that the saturation magnetic flux density decreases in many cases.
本発明の目的は、上述の従来技術の欠点を解消し、高飽
和磁束密度、低磁歪定数、高透磁率の特性を有する積層
磁性薄膜および上記積層磁性薄膜を用いた高密度磁気記
録用の磁気ヘッドを提供することにある。An object of the present invention is to solve the above-mentioned drawbacks of the prior art, and to provide a laminated magnetic thin film having the characteristics of high saturation magnetic flux density, low magnetostriction constant, and high magnetic permeability, and a magnetic material for high-density magnetic recording using the laminated magnetic thin film. The purpose is to provide the head.
本発明は、Fe薄膜およびFeを主成分とする合金薄膜
を、F e −N i系合金薄膜を介して積層構造とす
ることにより磁歪定数を調整する。The present invention adjusts the magnetostriction constant by forming an Fe thin film and an alloy thin film containing Fe as a main component into a laminated structure with an Fe--Ni alloy thin film interposed therebetween.
すなわち、Fe薄膜あるいはFeを主成分とする合金f
#膜にFe−Ni系合金薄膜を介して積層41マl造と
すると磁歪定数が増加し、上記積層構造の1周期の厚さ
を170〜1000人とすると磁歪定数を一2X10−
6から2X10−’の範囲とすることができる。That is, an Fe thin film or an alloy f mainly composed of Fe
# If the film is laminated with a Fe-Ni alloy thin film interposed in 41 layers, the magnetostriction constant will increase, and if the thickness of one period of the laminated structure is 170 to 1000, the magnetostriction constant will be -2X10-
It can range from 6 to 2X10-'.
さらに本発明の積層磁性薄膜を磁気ヘッドの磁気回路に
用いることにより、記録特性の優れた磁気ヘッドを得る
ことができる。Further, by using the laminated magnetic thin film of the present invention in a magnetic circuit of a magnetic head, a magnetic head with excellent recording characteristics can be obtained.
〔実施例1〕
第2図に示すようなデュアル・イオンビーム・スパッタ
リング装置21を用いて、Fe薄膜をパーマロイ薄膜を
介して積層構造として積層磁性薄膜を作製した。ターゲ
ット22としては125nnX 125mmX 5oa
tのFe(純度99.9%)を用い、ターゲット23と
しては同じ大きさのパーマロイ(NiatFsxo、重
量%)合金(純度99.9%)を用いた。薄膜作製は蒸
着用イオンガン24を用いてターゲット22あるいはタ
ーゲット23をイオン照射し、その時スパッタリングし
た粒子を基板ホルダー25上にセットした基板20の上
に蒸着することによって行った。ターゲット・ホルダー
26は回転することができ、ターゲット22およびター
ゲット23を交互にイオン照射するこにより磁性薄膜を
積層構造とすることができる。また積層磁性薄膜作製時
には基板照射用イオンガン27を用いて基板にイオンビ
ームを照射した。基板20としては磁歪定数測定用にコ
ーニング社製ホトセラム基板を用い、それ以外の特性の
測定用にはコーニング社製7059ガラス基板を用いた
。スパッタリングは以下の条件で行った。[Example 1] Using a dual ion beam sputtering apparatus 21 as shown in FIG. 2, a laminated magnetic thin film was produced in which an Fe thin film was laminated with a permalloy thin film interposed therebetween. Target 22 is 125nnX 125mmX 5oa
A permalloy (NiatFsxo, weight %) alloy (purity 99.9%) of the same size was used as the target 23. The thin film was produced by irradiating the target 22 or 23 with ions using the ion gun 24 for deposition, and then depositing the sputtered particles onto the substrate 20 set on the substrate holder 25. The target holder 26 can be rotated, and by alternately irradiating the targets 22 and 23 with ions, the magnetic thin film can be formed into a layered structure. Further, when producing the laminated magnetic thin film, the substrate was irradiated with an ion beam using the ion gun 27 for substrate irradiation. As the substrate 20, a photoceram substrate manufactured by Corning was used for measuring the magnetostriction constant, and a 7059 glass substrate manufactured by Corning was used for measuring other characteristics. Sputtering was performed under the following conditions.
イオンガス ・・・Ar装置内Arガス
圧力 ・・・2X10−”Pa蒸着用イオンガン
加速電圧 ・・・1200V蒸着用イオンガン加速電流
・・・120mAターゲット電流 ・・・
70mA基板照射用イオンガン加速電圧・・・200
v基板照射用イオンガン加速電流・・・ 40mAター
ゲット・基板間距離 ・・・127III11上記
条件でのFe薄膜の蒸着率は2.2人/sea、パーマ
ロイ薄膜の蒸着率は2.7人/see、であった。積層
磁性薄膜全体の膜厚は5000人一定として、パーマロ
イ中間層膜厚は50人一定とした。Ion gas... Ar gas pressure in Ar device... 2X10-''Pa ion gun acceleration voltage for evaporation... 1200V ion gun acceleration current for evaporation... 120 mA target current...
70mA ion gun acceleration voltage for substrate irradiation...200
v Ion gun acceleration current for substrate irradiation...40mA Target-substrate distance...127III11 Under the above conditions, the deposition rate of Fe thin film is 2.2 people/sea, the deposition rate of Permalloy thin film is 2.7 people/see, Met. The thickness of the entire laminated magnetic thin film was constant for 5000 people, and the thickness of the permalloy intermediate layer was constant for 50 people.
このようにして作製した積層磁性薄膜の断面図を第3図
に示す0本実施例では積層磁性薄膜は基板33上にFe
主磁性膜31およびパーマロイ中間層32が交互に堆積
した構造となっている。A cross-sectional view of the laminated magnetic thin film produced in this manner is shown in FIG.
It has a structure in which a main magnetic film 31 and a permalloy intermediate layer 32 are alternately deposited.
第3図におけるFe主磁性膜31の暦数と積層磁性薄膜
全体の磁歪定数との関係を第1図に示す。FIG. 1 shows the relationship between the calendar number of the Fe main magnetic film 31 in FIG. 3 and the magnetostriction constant of the entire laminated magnetic thin film.
同図の磁歪定数の層数依存性11に示すように。As shown in layer number dependence 11 of the magnetostriction constant in the same figure.
暦数が1、すなわちパーマロイ中間層を介さない単層の
膜の磁歪定数は−2,9XIO″″Bであった。The magnetostriction constant of the single-layer film with a calendar number of 1, that is, without a permalloy intermediate layer, was −2.9XIO″″B.
これにパーマロイ中間層を介して層数を増加させていく
と、積層磁性薄膜の磁歪定数は増加し、零に近づく0層
数を5〜30の範囲とすると磁歪定数は一2X10”−
B〜2X10−6の範囲となる。また層数を20とする
と磁歪定数はほぼ零となった。When the number of layers is increased through a permalloy intermediate layer, the magnetostriction constant of the laminated magnetic thin film increases.If the number of layers approaches zero in the range of 5 to 30, the magnetostriction constant becomes -2X10''-
The range is from B to 2X10-6. Moreover, when the number of layers was set to 20, the magnetostriction constant became almost zero.
なお、層数が30を越える膜の作製も試みたが、このよ
うな膜は基板からはく離してしまい、磁気特性を測定す
ることができなかった。Although an attempt was made to fabricate a film with more than 30 layers, such a film peeled off from the substrate, making it impossible to measure the magnetic properties.
第4図にFe主磁性膜の層数と積層磁性薄膜の保磁力と
の関係を示す、同図の磁化容易方向の保磁力41および
磁化困難方向の保磁力42のように、暦数が5層以上に
なると単層膜よりも保磁力が減少する。また、磁歪定数
がほぼ零となる20層の積層磁性薄膜では、磁化容易方
向の保磁力が7 、10 e、磁化困難方向の保磁力が
2.90eとなり、Feのみの単層膜と比べ良好な軟磁
気特性が得られた。また、層数が30の場合は層数20
とほぼ同じ保磁力を示した。Figure 4 shows the relationship between the number of layers of the Fe main magnetic film and the coercive force of the laminated magnetic thin film. When the film becomes more than one layer, the coercive force decreases compared to a single layer film. In addition, in a 20-layer laminated magnetic thin film with a magnetostriction constant of almost zero, the coercive force in the direction of easy magnetization is 7.10 e, and the coercive force in the direction of difficult magnetization is 2.90 e, which is better than a single layer film made only of Fe. Soft magnetic properties were obtained. Also, if the number of layers is 30, the number of layers is 20.
It showed almost the same coercive force.
第5図にFe主磁性膜の層数と積層磁性薄膜の比透磁率
(測定周波数5MH2)との関係を示す。FIG. 5 shows the relationship between the number of layers of the Fe main magnetic film and the relative magnetic permeability of the laminated magnetic thin film (measured at a frequency of 5 MH2).
同図の比透磁率の層数依存性51のように1層数が5以
上になると単層膜よりも比透磁率が高くなる。As shown in the dependence of relative magnetic permeability on the number of layers 51 in the figure, when the number of layers is five or more, the relative magnetic permeability becomes higher than that of a single layer film.
上述のように、Fe薄膜をパーマロイ薄膜を介して積層
型とした磁性薄膜は、その層数を増すに従って磁歪定数
が増加する。本実施例のように積層磁性薄膜の総膜厚が
5000人の場合、特に−2X10−6〜2 X 10
−6の範囲の磁歪定数を得るためには層数を5〜30、
すなわち積層構造の1周期を約170〜1000人の範
囲とする必要がある。またこのような積層磁性薄膜は低
保磁力。As described above, in a magnetic thin film in which Fe thin films are laminated with permalloy thin films interposed therebetween, the magnetostriction constant increases as the number of layers increases. When the total thickness of the laminated magnetic thin film is 5000 people as in this example, especially -2X10-6 to 2X10
In order to obtain a magnetostriction constant in the range of -6, the number of layers is 5 to 30,
That is, one period of the laminated structure needs to be in the range of about 170 to 1,000 people. In addition, this type of laminated magnetic thin film has a low coercive force.
高透磁率の特性を有する。また、磁歪定数がほぼ零であ
る層数20(周期約250人)の積層磁性薄膜の飽和磁
束密度は1.9Tであった。It has the property of high magnetic permeability. Further, the saturation magnetic flux density of a laminated magnetic thin film with 20 layers (period: about 250 layers) with a magnetostriction constant of almost zero was 1.9T.
また、積層磁性薄膜の総膜厚を340人、1μ膣。In addition, the total thickness of the laminated magnetic thin film was 340 people and 1μ vagina.
10μm、30μmとした場合についても1周期の厚さ
と磁歪定数との関係を調べた。その結果、1周期の厚さ
と磁歪定数との関係は総膜厚5000人の場合と同様で
あり、積層構造の1周期を170〜1000人とするこ
とにより磁歪定数の絶対値が2X10−6以下となるこ
とが明らかになった。The relationship between the thickness of one period and the magnetostriction constant was also investigated for the cases of 10 μm and 30 μm. As a result, the relationship between the thickness of one period and the magnetostriction constant is the same as in the case of a total film thickness of 5000 people, and by setting one period of the laminated structure to 170 to 1000 people, the absolute value of the magnetostriction constant is 2X10-6 or less. It became clear that.
すなわち、総膜厚340人〜30μmの本発明の積層磁
性薄膜は、積層構造の1周期を170〜1000人とす
ることにより2X10−8以下の絶対値を有するように
なる。That is, the laminated magnetic thin film of the present invention having a total thickness of 340 to 30 μm has an absolute value of 2×10 −8 or less by setting one period of the laminated structure to 170 to 1000 layers.
またさらに、主磁性膜としてFe 0.5vt%Ni
合金、Fe−0.5vt%C合金、Fe−0,7wt%
Rh合金などを用いた積層磁性薄膜を作製した。上記F
e系合金の磁歪定数はいずれも負の値であった。このよ
うなFe系合金を積層化した場合も積層化に件う磁歪定
数の変化はFe薄膜とほぼ同様であり、積層構造の1周
期の厚さを170〜1000人とすることにより、零に
近い磁歪定数を有する積層磁性薄膜が得ら九る。Furthermore, Fe 0.5vt%Ni is used as the main magnetic film.
Alloy, Fe-0.5vt%C alloy, Fe-0.7wt%
A laminated magnetic thin film using Rh alloy or the like was fabricated. Above F
The magnetostriction constants of the e-based alloys were all negative values. Even when such Fe-based alloys are laminated, the change in magnetostriction constant due to lamination is almost the same as that of Fe thin film, and by setting the thickness of one period of the laminated structure to 170 to 1000, it can be reduced to zero. A laminated magnetic thin film with similar magnetostriction constants can be obtained.
〔実施例2〕
本発明の、Feにパーマロイ合金を介して10層積層し
た積層磁性薄膜ないし従来の実用材料であるパーマロイ
(N i −19wt%Fe)合金薄膜を用いて第6図
に示す構造の垂直磁気記録用単磁極型磁気ヘッド71を
作製した。この磁気ヘッド71の作製工程を以下に述べ
る。[Example 2] The structure shown in FIG. 6 was prepared using the laminated magnetic thin film of the present invention in which 10 layers were laminated on Fe with permalloy alloy interposed therebetween, or the permalloy (N i -19wt%Fe) alloy thin film, which is a conventional practical material. A single-pole magnetic head 71 for perpendicular magnetic recording was manufactured. The manufacturing process of this magnetic head 71 will be described below.
第6図(a)に示すM n −Z nフェライト61お
よび高融点ガラス62からなる基板63を用い、その表
面に第6図(b)に示すように膜厚0.2μmの上記磁
性薄膜64をイオンビームスパッタリング法で作製した
。さらに、この上に接着用pb系ガラス膜(図示せず)
をイオンビームスパッタリング法により形成し、第6図
(a)に示す基板63と同等の基板を重ね合わせて45
0℃で30分間加熱し、上記pb系ガラス膜を溶融固着
させ、第6図(c)に示す主磁極ブロック65を作製し
た。そして第6図(d)に示すM n −Z nフェラ
イト66および高融点ガラス67からなる補助コアブロ
ック68を用意し、接合面70に上記と同様の接着用p
b系ガラス膜を形成した後、主6j1極ブロツク65を
補助コアブロック68の接合面70によって挟み、45
0℃で30分間加熱することにより、上記pb系ガラス
膜を容重固着させて接合ブロック69を作製した。次に
第6図(d)に示す2点鎖線部を切断し、第6図(e)
に示す垂直磁気記録用単磁極型磁気へラド71を得た。A substrate 63 made of Mn-Zn ferrite 61 and high melting point glass 62 shown in FIG. 6(a) is used, and the magnetic thin film 64 with a thickness of 0.2 μm is coated on the surface thereof as shown in FIG. 6(b). was fabricated using the ion beam sputtering method. Furthermore, a PB-based glass film (not shown) for adhesion is added on top of this.
was formed by an ion beam sputtering method, and a substrate 45 equivalent to the substrate 63 shown in FIG. 6(a) was superimposed.
The main pole block 65 shown in FIG. 6(c) was produced by heating at 0° C. for 30 minutes to melt and fix the PB glass film. Then, an auxiliary core block 68 made of Mn-Zn ferrite 66 and high melting point glass 67 shown in FIG.
After forming the b-based glass film, the main 6j 1-pole block 65 is sandwiched between the joint surfaces 70 of the auxiliary core block 68, and the 45
By heating at 0° C. for 30 minutes, the above-mentioned PB-based glass film was solidified to form a bonded block 69. Next, cut the two-dot chain line shown in Fig. 6(d), and then cut the part shown in Fig. 6(e).
A single-pole type magnetic helad 71 for perpendicular magnetic recording was obtained.
上述の工程によって作製した本発明の積層磁性薄膜を用
いたヘッドおよびパーマロイ薄膜を用いたヘッドの記録
特性をCo −Cr垂直磁気記録媒体を用いて測定した
。可成ヘッドにはパーマロイ薄膜を有するヘッドを用い
た。その結果、本発明の積層磁性薄膜を用いたヘッドは
、従来の実用材料であるパーマロイ合金薄膜を用いたヘ
ッドと比較して約5dB高い出力を示した。このように
本発明の強磁性合金を用いた磁気ヘッドは優れた記録特
性を有することが明らかとなった。The recording characteristics of the head using the laminated magnetic thin film of the present invention and the head using the permalloy thin film produced by the above steps were measured using a Co--Cr perpendicular magnetic recording medium. A head having a permalloy thin film was used as the removable head. As a result, the head using the laminated magnetic thin film of the present invention exhibited approximately 5 dB higher output than the head using the permalloy alloy thin film, which is a conventional practical material. As described above, it has been revealed that the magnetic head using the ferromagnetic alloy of the present invention has excellent recording characteristics.
以上詳細に説明したごとく、Fe系合金薄膜にFe−N
i系合金膜を介して作製した本発明の積層磁性薄膜は、
積層構造の1周期の厚さによって磁歪定数を制御するこ
とができる。すなわち1周期の厚さを170〜1000
人の範囲とすることにより、積層磁性薄膜の磁歪定数の
絶対値を2X10−B以下とすることができる。またこ
のような積層磁性薄膜は低保磁力、高透磁率の特性を有
する。さらに上記積層磁性薄膜を磁気ヘッドの磁気回路
の用いた本発明の磁気ヘッドは優れた記録特性を有する
。As explained in detail above, Fe-N is added to the Fe-based alloy thin film.
The laminated magnetic thin film of the present invention produced via an i-based alloy film is
The magnetostriction constant can be controlled by the thickness of one period of the laminated structure. In other words, the thickness of one period is 170 to 1000
By setting it within the human range, the absolute value of the magnetostriction constant of the laminated magnetic thin film can be set to 2×10 −B or less. Further, such a laminated magnetic thin film has characteristics of low coercive force and high magnetic permeability. Furthermore, the magnetic head of the present invention in which the above laminated magnetic thin film is used in the magnetic circuit of the magnetic head has excellent recording characteristics.
第1図は本発明の実施例1における積層型磁性薄膜の磁
歪定数と層数との関係を示すグラフ、第2図は本発明の
積層磁性薄膜の作製に用いたデュアル・イオンビーム・
スパッタリング装置の概略図、第3図は本発明の積層型
磁性薄膜の構造を示す断面図、第4図は本発明の積層型
磁性薄膜の保磁力と暦数との関係を示すグラフ、第5図
は本発明の積層型磁性薄膜の比透磁率と暦数との関係を
示すグラフ、第6図は本発明の磁気ヘッドの作製工程を
示す斜視図である。
21・・・デュアル・イオンビーム・スパッタリング装
置、22.23・・・ターゲット、24・・・蒸着用イ
オンガン、25・・・基板ホルダー、26・・・ターゲ
ットホルダー、27・・・基板照射用イオンガン、31
・・・Fa主磁性膜、32・・・パーマロイ中間層、3
3・・・基板、41・・・磁化容易方向の保磁力、42
・・・磁化困難方向の保磁力、51・・・比透磁率の層
数依存性、61.66−Mn−Znnフタイ1−162
゜67・・・高融点ガラス、63・・・基板、64・・
・磁性簿膜、65・・・主磁極ブロック、68・・・補
助コアブロック、69・・・接合ブロック、70・・・
接合面、71・・・垂直磁気記録用単磁極型磁気ヘッド
。
第 l 口
Iけ和滲さくバ)
も2I!1
零31!]
71 叡
第5記
45゛l 上ヒ31i鳥午/1.〜を掴古ζイオ2?’
フを件2第6 凹FIG. 1 is a graph showing the relationship between the magnetostriction constant and the number of layers of the laminated magnetic thin film in Example 1 of the present invention, and FIG. 2 is a graph showing the relationship between the magnetostriction constant and the number of layers of the laminated magnetic thin film of the present invention.
A schematic diagram of a sputtering apparatus, FIG. 3 is a cross-sectional view showing the structure of the laminated magnetic thin film of the present invention, FIG. 4 is a graph showing the relationship between coercive force and calendar number of the laminated magnetic thin film of the present invention, and FIG. The figure is a graph showing the relationship between the relative magnetic permeability and the calendar number of the laminated magnetic thin film of the invention, and FIG. 6 is a perspective view showing the manufacturing process of the magnetic head of the invention. 21...Dual ion beam sputtering device, 22.23...Target, 24...Ion gun for deposition, 25...Substrate holder, 26...Target holder, 27...Ion gun for substrate irradiation , 31
...Fa main magnetic film, 32...Permalloy intermediate layer, 3
3... Substrate, 41... Coercive force in the direction of easy magnetization, 42
... Coercive force in direction of difficult magnetization, 51 ... Dependence of relative magnetic permeability on number of layers, 61.66-Mn-Znn frame 1-162
゜67...High melting point glass, 63...Substrate, 64...
-Magnetic film, 65...Main pole block, 68...Auxiliary core block, 69...Joining block, 70...
Joint surface, 71... Single-pole magnetic head for perpendicular magnetic recording. Part l 口I け和滲さくば)も2I! 1 zero 31! ] 71 Ei No. 5 45゛l Jōhi 31i Torigo/1. Grab the old ζio2? '
2nd 6th concave
Claims (1)
e−Ni系合金薄膜を介して積層構造とした磁性薄膜に
おいて、上記積層構造の1周期の厚さが170〜100
0Åの範囲であることを特徴とする積層磁性薄膜。 2、磁性薄膜を磁気回路の少なくとも一部に用いる磁気
ヘッドにおいて、上記磁性薄膜は、Fe薄膜あるいはF
eを主成分とする合金薄膜にFe−Ni系合金薄膜を介
して積層構造とした磁性薄膜であり、かつ上記積層構造
の1周期の厚さが170〜1000Åの範囲であること
を特徴とする積層磁性薄膜を用いた磁気ヘッド。[Claims] 1. F in Fe thin film or alloy thin film mainly composed of Fe.
In a magnetic thin film having a laminated structure via an e-Ni alloy thin film, the thickness of one period of the laminated structure is 170 to 100 mm.
A laminated magnetic thin film characterized in that the thickness is in the range of 0 Å. 2. In a magnetic head that uses a magnetic thin film in at least a part of the magnetic circuit, the magnetic thin film is an Fe thin film or an F
A magnetic thin film having a laminated structure with an alloy thin film mainly composed of e and an Fe-Ni alloy thin film interposed therebetween, and characterized in that the thickness of one period of the laminated structure is in the range of 170 to 1000 Å. A magnetic head using laminated magnetic thin films.