JPS63275106A - Magnetic thin film and manufacture thereof - Google Patents
Magnetic thin film and manufacture thereofInfo
- Publication number
- JPS63275106A JPS63275106A JP10974787A JP10974787A JPS63275106A JP S63275106 A JPS63275106 A JP S63275106A JP 10974787 A JP10974787 A JP 10974787A JP 10974787 A JP10974787 A JP 10974787A JP S63275106 A JPS63275106 A JP S63275106A
- Authority
- JP
- Japan
- Prior art keywords
- magnetic
- thin film
- film
- permalloy
- magnetic thin
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Pending
Abstract
Description
【発明の詳細な説明】
〔産業上の利用分野〕
この発明は、例えば、薄膜磁気ヘッドの磁極材料である
ニッケルー鉄合金(Ni−Fe )系パーマロイの高透
磁率スパッタ膜などとして好適に用いることのできる磁
性薄膜及びその製造方法に関するものである。[Detailed Description of the Invention] [Industrial Application Field] The present invention can be suitably used, for example, as a high magnetic permeability sputtered film of nickel-iron alloy (Ni-Fe) based permalloy, which is a magnetic pole material of a thin-film magnetic head. The present invention relates to a magnetic thin film that can be made and a method for manufacturing the same.
磁気ヘッド用の磁性材料としては、透磁率の高いことが
要求されることがらNi−Fe系の合金であるパーマロ
イがよく知られており、従来は、例えば、公開特許公報
昭55−82793号などに示された電気メツキ法によ
り作成されていた。第5図には、電気メツキ法により、
作成したパーマロイ薄膜の磁気特性の例として、B−H
ルーグ曲線を示す。(印加磁界はsoe、)このような
方法では、透磁率が約3000の磁性膜が得られる。し
かしながら、高記録密度領域において、十分な記録再生
特性を得るためには、より高透磁率の磁性膜が記録再生
効率の点で有利であり必要であるばかりでなく、従来の
メッキ膜を用いたヘッド製造では、例えば、公開特許公
報昭55−84019号などに示されているようにヨー
ク部分において、コア厚を厚くして、磁気的な効率を上
げる必要があった。また、高記録密度領域では、ヘッド
の使用される周波数が高くなるため、周波数特性の良好
なヘッドの作成も望まれている。さらに、メッキ法では
、均一な特性の磁性膜を再現性よく大量に作成すること
がメッキ浴の管理上からも困難であり、歩留まりの低下
する要因にもなりかねないため、生産性にも乏しい方式
である。Permalloy, which is a Ni-Fe alloy, is well known as a magnetic material for magnetic heads because it is required to have high magnetic permeability. It was created using the electroplating method shown in . Figure 5 shows that by the electroplating method,
As an example of the magnetic properties of the permalloy thin film created, B-H
Showing the Roog curve. (The applied magnetic field is soe.) With this method, a magnetic film with a magnetic permeability of about 3000 is obtained. However, in order to obtain sufficient recording and reproducing characteristics in the high recording density area, a magnetic film with higher magnetic permeability is not only advantageous and necessary in terms of recording and reproducing efficiency, but also In head manufacturing, it is necessary to increase the core thickness in the yoke portion to increase magnetic efficiency, as shown in, for example, Japanese Patent Publication No. 55-84019. Furthermore, in a high recording density area, the frequency at which the head is used increases, so it is also desired to create a head with good frequency characteristics. Furthermore, with the plating method, it is difficult to produce a large quantity of magnetic films with uniform characteristics with good reproducibility in terms of plating bath management, which can lead to a decrease in yield, resulting in poor productivity. It is a method.
従来の薄膜磁気ヘッドの磁極材料であるパーマロイ膜な
どの磁性薄膜は以上のようにメッキ成膜されているので
、薄膜磁気ヘッドに用いる場合、ヨーク部分において、
コア厚を厚くして磁気的な効率を上げることが必要で、
また高記録密度領域では、十分な記録再生特性が得られ
ず、また、メッキ法では、再現性よく均一な特性の膜を
得ることがむずかしいという問題点があった。Magnetic thin films such as permalloy films, which are the magnetic pole materials of conventional thin-film magnetic heads, are plated as described above, so when used in thin-film magnetic heads, the yoke part
It is necessary to increase the magnetic efficiency by increasing the core thickness.
Further, in the high recording density region, sufficient recording and reproducing characteristics cannot be obtained, and the plating method has the problem that it is difficult to obtain a film with uniform characteristics with good reproducibility.
この発明は上記のような問題点を解消するためになされ
たもので、高記録密度領域においても十分な記録再生特
性を実現できる均一な特性の薄膜磁気ヘッドの磁極性の
パーマロイ磁性薄膜などとして好ましく用いることので
きる高透磁率の磁性薄膜及びその製造方法を得ることを
目的とする。This invention was made to solve the above-mentioned problems, and is preferable as a permalloy magnetic thin film with magnetic polarity for a thin-film magnetic head with uniform characteristics that can realize sufficient recording and reproducing characteristics even in a high recording density area. The purpose is to obtain a magnetic thin film with high magnetic permeability that can be used and a method for manufacturing the same.
この発明に係る磁性薄膜は、パーマロイなどの磁性体と
アルミナなどの非磁性の絶縁体膜とを交互にスパッタに
より積層したものである。また、その製造方法は、上記
スパッタを40〜60Oe、の磁場中で行うようにした
ものである。The magnetic thin film according to the present invention is a film in which a magnetic material such as permalloy and a non-magnetic insulating film such as alumina are alternately laminated by sputtering. Moreover, the manufacturing method is such that the above-mentioned sputtering is performed in a magnetic field of 40 to 60 Oe.
この発明における磁性薄膜は、非磁性の絶縁体膜を介し
た積層構造により、各層の磁性膜の磁化の方向を交互に
逆向きにすることができ、透磁率を大きくする。The magnetic thin film according to the present invention has a laminated structure with nonmagnetic insulating films interposed therebetween, so that the direction of magnetization of the magnetic films in each layer can be alternately reversed, thereby increasing magnetic permeability.
以下、この発明の一実施例を図について説明する。第1
図は、本発明の一実施例の高透磁率パーマロイ・スパッ
タ膜の断面構造を示したもので、図において、(11は
基板、(21はこの基板上にスパン夕蒸着されたパーマ
ロイ、(3)は磁化容易軸方向、(4)は絶縁体膜であ
る。第2図は、上記実施例の高透磁率パーマロイ・スパ
ッタ膜の作成方法における成膜工程時の基板配置を示す
概観図で、図において、(1)は基板、(5)は磁石で
ある。第3図は、上記実施例の高透磁率パーマロイ・ス
パッタ膜の作成方法における熱処理工程時の基板配置を
示す概観図で、図において、(1)は基板、(3)は磁
化容易軸、(5)は磁石である。第4図は、上記実施例
の高透磁率パーマロイ・スパッタ膜の磁気特性を示すB
−Hループ曲線である。An embodiment of the present invention will be described below with reference to the drawings. 1st
The figure shows the cross-sectional structure of a high magnetic permeability permalloy sputtered film according to an embodiment of the present invention. ) is the easy axis direction of magnetization, and (4) is the insulating film. Fig. 2 is an overview diagram showing the substrate arrangement during the film forming process in the method for producing the high magnetic permeability permalloy sputtered film of the above embodiment. In the figure, (1) is a substrate, and (5) is a magnet. Fig. 3 is an overview diagram showing the substrate arrangement during the heat treatment process in the method for producing a high magnetic permeability permalloy sputtered film of the above embodiment. , (1) is the substrate, (3) is the axis of easy magnetization, and (5) is the magnet. Figure 4 shows the magnetic properties of the high permeability permalloy sputtered film of the above example.
-H loop curve.
次に、上記本発明の一実施例になる高透磁率パーマロイ
・スパッタ膜の構造、作成方法、性能を説明する。磁気
ヘッド用の磁極材料としては、透磁率の高いことが要求
されることから、一般には、磁性体の面内における磁化
の向きを一定の方向に揃える(−軸異方性を誘起する。Next, the structure, manufacturing method, and performance of the high magnetic permeability permalloy sputtered film according to an embodiment of the present invention will be explained. Since magnetic pole materials for magnetic heads are required to have high magnetic permeability, the in-plane magnetization direction of the magnetic material is generally aligned in a certain direction (-inducing anisotropy in the negative axis).
)ことで、高透磁率化を図っている。そのため、一定の
方向に磁場を印加した状態で成膜することにより、−軸
異方性を誘起している。因みに従来技術のメッキ膜では
、数百Oe、の磁場中で成膜している。しかしながら、
スパッタ方式では、大きな磁場を印加すると、放電が安
定して起こらないため、外部磁場の大きさは数十Oe、
が限界である。一方、小さな磁場でスパッタ膜を得ると
、外部磁場の大きさが十分でないため、ある大きさ以上
の膜厚になると、−軸異方性が誘起されない。本発明者
らの実験では、膜厚が、111m以上になると、−軸異
方性が誘起されにくくなり、たとえ、−軸異方性が誘起
されたとしても、得られた磁性膜の透磁率は、メッキ膜
と同様、もしくは、それ以下であった。), thereby achieving high magnetic permeability. Therefore, -axis anisotropy is induced by forming a film while applying a magnetic field in a fixed direction. Incidentally, the plating film of the prior art is formed in a magnetic field of several hundred Oe. however,
In the sputtering method, if a large magnetic field is applied, discharge will not occur stably, so the magnitude of the external magnetic field is several tens of Oe,
is the limit. On the other hand, when a sputtered film is obtained with a small magnetic field, the external magnetic field is not large enough, so that -axis anisotropy is not induced when the film thickness exceeds a certain value. In experiments conducted by the present inventors, when the film thickness becomes 111 m or more, -axis anisotropy is difficult to be induced, and even if -axis anisotropy is induced, the magnetic permeability of the obtained magnetic film is was the same as or lower than that of the plated film.
本発明は上記様々の問題を克服してなされたもので、非
磁性の絶縁体膜を介して磁性膜を積層構造にして一軸異
方性が誘起されやすくなるようにしたものである。すな
わち、積層構造にすることで、磁性層間の面内磁化の方
向が、例えば、第1図に示すように、交互に反転するよ
うな構造の磁性膜を作成すれば、膜全体としては、−軸
異方性が誘起されているので、高透磁率化が期待できる
。The present invention has been made to overcome the various problems described above, and has a laminated structure of magnetic films with non-magnetic insulating films interposed therebetween, so that uniaxial anisotropy is easily induced. That is, if a magnetic film is created with a laminated structure in which the direction of in-plane magnetization between the magnetic layers is alternately reversed, as shown in FIG. 1, for example, the film as a whole will have - Since axial anisotropy is induced, high magnetic permeability can be expected.
具体的には、パーマロイと非磁性の絶縁体膜であるA1
0 を、それぞれ、1000〜2000Å、100〜5
00Aずつ交互に第2図の如(40〜60Oe、の磁場
中でスパッタ蒸着によって積層し、成膜後、第3図に示
すようにスパッタ時の磁場の方向に垂直な方向の40〜
100Oe、の磁場中で、かつ、好ましくは200〜2
50℃の雰囲気中で1時間以上熱処理することにより、
透磁率が約5000の高透磁率ノパーマロイ・スパッタ
膜が、再現性よく得うれた。また、得られた高透磁率パ
ーマロイ・スパンpgco膜応力は、いずれも、5 X
10” dyn / crIL2以上であった。スパ
ッタ条件を変化させて、膜応力がs x t o9dy
n / cm2以下の磁性膜を作成したが、得られた膜
の透磁率は、いずれも、メッキ膜と同等、もしくは、そ
れ以下であった。従って、パーマロイ・スパッタ膜の磁
気特性は、応力によって、誘起されていると考えられ、
5 X 10’dyn/α2以上の膜応力が高透磁率化
には、必要である。Specifically, permalloy and A1, which is a non-magnetic insulating film,
0 to 1000 to 2000 Å and 100 to 5
00A is alternately laminated by sputter deposition in a magnetic field of 40 to 60 Oe as shown in Fig. 2, and after film formation, as shown in Fig.
in a magnetic field of 100 Oe, and preferably 200 to 2
By heat-treating in an atmosphere of 50°C for more than 1 hour,
A high permeability Nopermalloy sputtered film with a magnetic permeability of about 5000 was obtained with good reproducibility. In addition, the stress of the obtained high permeability permalloy spun PGCO film is 5
The film stress was 10" dyn/crIL2 or more by changing the sputtering conditions.
Magnetic films of n/cm2 or less were created, but the magnetic permeability of the obtained films was equal to or lower than that of the plated film. Therefore, the magnetic properties of permalloy sputtered films are thought to be induced by stress.
A film stress of 5 x 10'dyn/α2 or more is necessary to increase magnetic permeability.
さらに、スパッタ蒸着の際に基板を加熱することは好ま
しいことであり、例えば100〜150℃に基板を加熱
した状態で行うと、得られる磁性膜の透磁率は、さらに
大きくなり、この場合には第4図に示すように透磁率が
約7000のパーマロイ・スパッタ膜が得られた。Furthermore, it is preferable to heat the substrate during sputter deposition; for example, if the substrate is heated to 100 to 150°C, the magnetic permeability of the resulting magnetic film will be even higher; As shown in FIG. 4, a permalloy sputtered film having a magnetic permeability of about 7000 was obtained.
なお、非磁性の絶縁体膜として、アルミナ(A1203
)を用いたが、特にこのものに限定されず、種々のもの
を用いることができる。例えばSiO□、TiO2など
も好ましく用いることができる。Note that alumina (A1203
) was used, but the invention is not particularly limited to this one, and various other ones can be used. For example, SiO□, TiO2, etc. can also be preferably used.
また、各磁性体膜の磁化の方向は一層毎に逆向きとした
ものでなくともよく、複数層毎、例えば5層毎でも差支
えない。Further, the direction of magnetization of each magnetic film does not have to be reversed for each layer, but may be set for every plurality of layers, for example every 5 layers.
また、上記実施例では、磁性体はパーマロイであったが
、これに限定されるものでないことは勿論であり、たと
えばコバルト系、鉄系、あるいはその他の磁性材料でも
よい。また、上記実施例では、産業上の利用分野として
、薄膜磁気ヘッドの磁極材料の場合について説明したが
、磁気センサ、バルクヘッドや他の磁気デバイスであっ
てもよく、上記実施例と同様の効果を奏する。Further, in the above embodiment, the magnetic material is permalloy, but it is needless to say that it is not limited to this, and may be, for example, cobalt-based, iron-based, or other magnetic materials. Further, in the above embodiment, the case of the magnetic pole material of a thin film magnetic head was explained as an industrial application field, but it may also be applied to a magnetic sensor, a bulk head, or other magnetic device, and the same effect as in the above embodiment may be obtained. play.
以上のように、この発明によれば磁性体膜と非磁性の絶
縁体膜とをスパッタにより交互に積層したので、磁気特
性の丁ぐれた磁性薄膜が得られる効果がある。また、製
造に際しては40〜60Oe、の磁場中で磁性体膜と非
磁性体膜を交互にスパッタ成膜することにより、−軸異
方性の誘起も容易であり、透磁率の大きい磁性薄膜を製
造できるという効果がある。As described above, according to the present invention, since magnetic films and non-magnetic insulating films are alternately laminated by sputtering, a magnetic thin film with well-balanced magnetic properties can be obtained. In addition, during manufacturing, by alternately sputtering magnetic films and non-magnetic films in a magnetic field of 40 to 60 Oe, -axis anisotropy can be easily induced, and a magnetic thin film with high magnetic permeability can be produced. It has the advantage of being manufacturable.
第1図は、この発明の一実施例による高透磁率パーマロ
イ・スパッタ膜の積層構造を示す断面図、第2図は、こ
の発明の一実施例による高透磁率パーマロイ・スパッタ
膜の作成方法における成膜工程時の基板配置を示す概観
図、第3図は、実施例の方法における熱処理工程時の基
板配置を示す概観図、第4図は、上記実施例の高透磁率
パーマロイ・スパッタ膜の磁気特性を示すB−Hループ
曲線図、第5図は、従来のパーマロイ・メッキ膜の磁気
特性を示すB−Hループ曲線図である。
(1)は基板、(2)は磁性体膜としてのパーマロイ、
(3)は磁化容易軸方向、(4)は絶縁体膜である。
なお、図中、同一符号は同一、又は相当部分を示す。
1:丼才反
21石数J+−生イ本川喝()ぐマ0す4、絶オつ4イ
本月ダ(FIG. 1 is a cross-sectional view showing the laminated structure of a high permeability permalloy sputtered film according to an embodiment of the present invention, and FIG. FIG. 3 is an overview diagram showing the substrate arrangement during the film forming process. FIG. 3 is an overview diagram showing the substrate arrangement during the heat treatment process in the method of the example. FIG. FIG. 5 is a B-H loop curve diagram showing the magnetic characteristics of a conventional permalloy plated film. (1) is a substrate, (2) is permalloy as a magnetic film,
(3) is the easy axis direction of magnetization, and (4) is the insulator film. In addition, in the figures, the same reference numerals indicate the same or equivalent parts. 1: Donzai anti 21 koku number J + - Namai Honkawa Osaka ()guma 0su 4, Zetsuotsu 4i Honzuki da (
Claims (9)
交互に積層してなることを特徴とする磁性薄膜。(1) A magnetic thin film characterized by being formed by alternately laminating a magnetic film and a nonmagnetic insulating film by sputtering.
て構成されるパーマロイであり、このパーマロイと非磁
性の絶縁体の各スパッタ膜の厚さがそれぞれ、1000
〜2000Å、100〜500Åであることを特徴とす
る特許請求の範囲第1項記載の磁性薄膜。(2) The magnetic material is permalloy composed of nickel (Ni) and iron (Fe), and the thickness of each sputtered film of this permalloy and non-magnetic insulator is 1000 mm.
The magnetic thin film according to claim 1, wherein the magnetic thin film has a thickness of 100 to 500 Å.
0〜83.0%、鉄(Fe)19.0%〜17.0%に
よって構成されたものであることを特徴とする特許請求
の範囲第2項記載の磁性薄膜。(3) Permalloy has a weight ratio of nickel (Ni) of 81.
3. The magnetic thin film according to claim 2, wherein the magnetic thin film is composed of 0 to 83.0% iron (Fe) and 19.0% to 17.0% iron (Fe).
毎に交互に逆向きであることを特徴とする特許請求の範
囲第1項ないし第3項の何れかに記載の磁性薄膜。(4) Magnetism according to any one of claims 1 to 3, characterized in that the in-plane magnetization of the magnetic film of each layer is alternately opposite for each layer or layers. Thin film.
O_2の内の何れか一つ若しくは其の混合物によって構
成されることを特徴とする特許請求の範囲第1項ないし
第4項の何れかに記載の磁性薄膜。(5) The insulator film is made of Al_2O_3, SiO_2, Ti
The magnetic thin film according to any one of claims 1 to 4, characterized in that it is composed of any one of O_2 or a mixture thereof.
磁場中で交互にスパッタ蒸着することを特徴とする磁性
薄膜の製造方法。(6) A method for producing a magnetic thin film, which comprises alternately sputter-depositing a magnetic material and a non-magnetic insulator in a magnetic field of 40 to 60 Oe.
℃の加熱状態であることを特徴とする特許請求の範囲第
6項記載の磁性薄膜の製造方法。(7) During sputter deposition, the substrate temperature is 100 to 150
7. The method of manufacturing a magnetic thin film according to claim 6, wherein the heating is performed at a temperature of .degree.
方向の40〜100Oe、の磁場中で、1時間以上熱処
理することを特徴とする特許請求の範囲第6項または第
7項記載の磁性薄膜の製造方法。(8) Magnetic properties according to claim 6 or 7, characterized in that after sputter deposition, heat treatment is performed for 1 hour or more in a magnetic field of 40 to 100 Oe in a direction perpendicular to the magnetic field during sputtering. Method for manufacturing thin films.
を特徴とする特許請求の範囲第8項記載の磁性薄膜の製
造方法。(9) The method for manufacturing a magnetic thin film according to claim 8, wherein the heat treatment is performed in an atmosphere of 200 to 250°C.