JP7352233B2 - Methane purification catalyst with resistance to sulfur poisoning - Google Patents
Methane purification catalyst with resistance to sulfur poisoning Download PDFInfo
- Publication number
- JP7352233B2 JP7352233B2 JP2019173438A JP2019173438A JP7352233B2 JP 7352233 B2 JP7352233 B2 JP 7352233B2 JP 2019173438 A JP2019173438 A JP 2019173438A JP 2019173438 A JP2019173438 A JP 2019173438A JP 7352233 B2 JP7352233 B2 JP 7352233B2
- Authority
- JP
- Japan
- Prior art keywords
- methane
- atoms
- atom
- shows
- pdo
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Active
Description
本発明は、耐硫黄被毒性を有するメタン浄化触媒に関し、詳しくは、メタン浄化活性を損なうことなく、硫黄被毒を抑制することができる排ガス浄化用途に好適な耐硫黄被毒性を有するメタン浄化触媒に関するものである。 The present invention relates to a methane purification catalyst that is resistant to sulfur poisoning, and more specifically, a methane purification catalyst that is resistant to sulfur poisoning and is suitable for exhaust gas purification and is capable of suppressing sulfur poisoning without impairing methane purification activity. It is related to.
天然ガスを燃料とする熱機関において、運転時で完全燃焼しなかった場合や、運転停止時には、排ガス中にメタンが残留する。メタンは温室効果ガス(二酸化炭素の25倍)であるため大気排出前に浄化する必要がある。ここで、メタンの浄化とは、メタンを酸化して炭化水素を除去することをいう(以下、同様)。 In heat engines that use natural gas as fuel, methane remains in the exhaust gas when combustion does not occur completely during operation or when operation is stopped. Methane is a greenhouse gas (25 times more potent than carbon dioxide) and must be purified before it can be released into the atmosphere. Here, purification of methane means oxidizing methane to remove hydrocarbons (the same applies hereinafter).
排ガス中のメタンの浄化は、メタンより無害かつ地球温暖化係数の低い二酸化炭素と水へ変換する次の酸化反応が望ましい。 The following oxidation reaction, which converts methane in exhaust gas into carbon dioxide and water, which is more harmless and has a lower global warming potential than methane, is desirable.
CH4 + 2O2→ CO2 + 2H2O
現在、メタン浄化のメタン浄化触媒として酸化パラジウムが主に用いられている(特許文献1~5等)。しかし、脱硫された天然ガスにも微量の硫黄が含まれ、または、人為的に加える付臭剤にも硫黄が含まれ、メタン浄化触媒としての酸化パラジウムの触媒寿命を著しく損なう硫黄被毒を起こすという問題があった。
CH 4 + 2O 2 → CO 2 + 2H 2 O
Currently, palladium oxide is mainly used as a methane purification catalyst for methane purification (
そこで、本発明者らは、酸化パラジウムのメタン浄化における耐硫黄被毒を低減するため、硫黄被毒およびメタン活性の電子・原子レベルの機構の検討を行い、その結果を非特許文献1において報告した。
Therefore, in order to reduce the resistance to sulfur poisoning in methane purification of palladium oxide, the present inventors investigated the electronic and atomic level mechanisms of sulfur poisoning and methane activity, and reported the results in Non-Patent
上記非特許文献1では、メタン浄化における耐硫黄被毒触媒のモデル表面として、酸化パラジウムの安定に出現しうるPdO(101)面に着目した。図1はPdO(101)面の格子構造を示し、左側の図が側面図、右側の図が上面図である。薄い大きな灰色球はPd原子、濃い小さな灰色球は酸素原子を表す。最表面には、3つの酸素原子が配位したPd原子(以後Pd(3f)と表記)と4つの酸素原子が配位したPd原子(以後Pd(4f)と表記)が存在することが特徴である。図1の側面図と上面図にそれぞれの酸素配位面を四角で表した。前者は表面に垂直、後者は表面平行面よりわずかに傾斜している。
Non-Patent
各原子の局所状態密度を図2に示す。濃い実線がPdO(101)表面原子Pd(3f)の局所状態密度であり、薄い実線がPdO(101)表面原子Pd(4f)の局所状態密度である。比較のため金属のPd(211)表面原子の状態密度も示した。特徴的な電子状態としてフェルミレベル(EF)より高エネルギー側に現れた非占有状態ピークがあげられる。解析の結果、それらはPd(3f)では、表面垂直方向に延びたdzz軌道に、Pd(4f)では、隣接する酸素原子との間のdyz軌道による反結合軌道に帰属することが分かった。 Figure 2 shows the local density of states of each atom. The dark solid line is the local density of states of Pd(3f), an atom on the PdO(101) surface, and the thin solid line is the local density of states of Pd(4f), an atom on the PdO(101) surface. For comparison, the density of states of the surface atoms of the metal Pd(211) is also shown. A characteristic electronic state is an unoccupied state peak that appears on the higher energy side than the Fermi level (E F ). As a result of analysis, it was found that in Pd(3f), they belong to the d zz orbital extending perpendicular to the surface, and in Pd(4f), they belong to the antibonding orbital due to the d yz orbital between adjacent oxygen atoms. Ta.
図3の(a)にメタンの最安定吸着状態を求めた結果を示す。上側が上面図、下側が側面図である。また、図3の(b)にメタン分子が表面に安定に吸着するために必要な電子遷移(供与(donation))に関与する電子軌道を示し、図3の(c)にメタン活性に寄与する電子遷移(逆供与(back donation)に関与する電子軌道を示す。ここで、メタン活性とは、メタンから水素が取れやすくなった状態になることをいう(以下、同様)。メタン分子は、一つのPd(3f)上に吸着し、表面側のC-H結合距離が1.118Åに延び、活性化されていることが分かった。なお、表面とは反対側のC-H結合距離は1.095Åと気相中の1.097Åからほとんど変化していなかった。吸着時の電子状態を解析したところ。メタン分子のσ結合分子軌道からPd(3f)の非占有dzzへ電子供与がなされ、分子-表面間共有結合が生じ分子吸着状態を安定化させ、Pd(3f)の占有dyz軌道からメタンの表面側のC-H反結合σ*軌道に電子供与がなされ、C-H結合を弱めるメタン活性が起こっていることが分かった。 FIG. 3(a) shows the results of determining the most stable adsorption state of methane. The upper side is a top view, and the lower side is a side view. In addition, Figure 3 (b) shows the electron orbits involved in the electronic transition (donation) necessary for the stable adsorption of methane molecules to the surface, and Figure 3 (c) shows the electron orbits that contribute to methane activity. Shows the electron orbitals involved in electronic transition (back donation).Methane activity here refers to a state in which hydrogen can be easily removed from methane (the same applies hereinafter).Methane molecules are It was found that the CH bond distance on the surface side was extended to 1.118 Å, indicating that it was activated.The CH bond distance on the opposite side from the surface was 1.095 Å, indicating that it was activated. There was almost no change from 1.097 Å.The electronic state during adsorption was analyzed.Electrons were donated from the σ-bond molecular orbital of the methane molecule to the unoccupied d zz of Pd(3f), forming a covalent bond between the molecule and the surface. It was found that methane activity occurs, which stabilizes the molecular adsorption state and donates electrons from the occupied d yz orbital of Pd(3f) to the CH antibonding σ* orbital on the surface side of methane, weakening the CH bond. Ta.
図4に、活性化された表面側のC-H結合を切る反応(1)と、反対側の非活性化C-Hを切る反応(2)の反応経路と活性化障壁を調べた結果を示す。図中、TS1が吸着メタン分子のC-Hの内、Pd(3f)側の活性化されたC-Hを切る反応(1)の活性化障壁であり、TS2が非活性化C-Hを切る反応(2)の活性化障壁である。Pd(3f)側の活性化されたC-Hを切る反応(1)の活性化障壁は0.66eVと低く、容易におこる反応であることがわかった。これがPdOのメタン浄化触媒の最も重要な素反応過程である。 Figure 4 shows the results of investigating the reaction pathway and activation barrier for reaction (1), which cuts the C-H bond on the activated surface side, and reaction (2), which cuts the non-activated C-H bond on the opposite side. In the figure, TS1 is the activation barrier for reaction (1) that cuts activated C-H on the Pd(3f) side among the C-H of adsorbed methane molecules, and TS2 is the activation barrier for reaction (2) that cuts non-activated C-H. It is an activation barrier. The activation barrier for reaction (1), which cuts activated C-H on the Pd(3f) side, was as low as 0.66 eV, and it was found that this reaction occurs easily. This is the most important elementary reaction process of PdO as a methane purification catalyst.
次に、硫黄が酸化され二酸化硫黄SO2として触媒表面に接近し吸着酸化する反応を調べた結果を図5に示す。図5には、Eley-Rideal機構、Langmuir Hinshelwod機構、Mars-van Krevelen機構の3種類の機構の反応経路を調べた結果を示した。酸素分子解離吸着の遷移状態TS-ERを経る反応経路(下図では点線)がEley-Rideal機構のもの、遷移状態TS-LHを経る反応経路(下図では実線)がLangmuir Hinshelwod機構のもの、酸素分子の解離を伴わずPdO表面の酸素を奪う反応経路(下図では破線)がMars-van Krevelen機構のものである。図5の上図は、各機構の反応経路における原子位置の変遷を示し、図5の下図は自由エネルギーの変化を示した。各機構の反応経路で自由エネルギーの高い方が400℃の場合、低い方が絶対零度の場合である。 Next, we investigated the reaction in which sulfur is oxidized and approaches the catalyst surface as sulfur dioxide SO 2 and is adsorbed and oxidized. The results are shown in FIG. Figure 5 shows the results of investigating the reaction pathways of three types of mechanisms: Eley-Rideal mechanism, Langmuir Hinshelwod mechanism, and Mars-van Krevelen mechanism. The reaction route (dotted line in the figure below) that goes through the transition state TS-ER of dissociative adsorption of oxygen molecules is the Eley-Rideal mechanism, and the reaction route that goes through the transition state TS-LH (solid line in the figure below) is the Langmuir Hinshelwod mechanism, and the oxygen molecule The Mars-van Krevelen mechanism is the reaction pathway (dashed line in the figure below) that deprives oxygen from the PdO surface without dissociating. The upper diagram in FIG. 5 shows changes in atomic positions in the reaction paths of each mechanism, and the lower diagram in FIG. 5 shows changes in free energy. In the reaction path of each mechanism, the higher free energy is at 400°C, and the lower is at absolute zero.
比較の結果、触媒表面に飛来したSO2は、表面の酸素を反応に用いるMars-van Krevelen機構で容易に酸化しSO4になることが見いだされた。そのとき、飛来したSO2が表面に吸着するには、隣接する2個のPd(3f)と、それに隣接する1個のPd(4f)の計3個の表面Pd原子が必要なことが分かった。 As a result of the comparison, it was found that SO 2 that came to the catalyst surface was easily oxidized to SO 4 using the Mars-van Krevelen mechanism, which uses oxygen on the surface for the reaction. At that time, it was found that in order for the incoming SO 2 to be adsorbed on the surface, a total of three surface Pd atoms, two adjacent Pd(3f) and one adjacent Pd(4f), are required. Ta.
O2、CH4、SO2から二種を選んだ混合ガス下における熱力学的に安定な表面を調査した結果を図6に示す。縦軸と横軸はそれぞれのガス種の化学ポテンシャルΔμで、温度が400℃の場合の分圧換算を併記した。それぞれの領域は、表示した化学式の分子が吸着した場合が安定な化学ポテンシャルの領域を表す。*は、分子が吸着しない清浄表面が安定であることを示す。☆(白抜き☆記号は)は、典型的な排ガス実験条件のガス分圧(PCH_4 = 10-3 atm、PO_2 = 0.20 atm、PSO_2 = 5x10-6 atm)環境を示す。メタンと酸素の共存下(図6の上図)、およびメタンと二酸化硫黄の共存下(図6の中図)では、清浄表面が熱力学的に安定でメタン活性が維持されることが見いだされた。 Figure 6 shows the results of investigating thermodynamically stable surfaces under a mixed gas of two selected from O 2 , CH 4 , and SO 2 . The vertical and horizontal axes represent the chemical potential Δμ of each gas species, and the partial pressure conversion at a temperature of 400°C is also shown. Each region represents a region of stable chemical potential when molecules of the indicated chemical formula are adsorbed. * indicates that a clean surface where molecules are not adsorbed is stable. The ☆ (open ☆ symbol) indicates the gas partial pressure (P CH_4 = 10 -3 atm, P O_2 = 0.20 atm, P SO_2 = 5x10 -6 atm) environment under typical exhaust gas experimental conditions. It was found that the clean surface is thermodynamically stable and methane activity is maintained under the coexistence of methane and oxygen (upper panel in Figure 6) and under the coexistence of methane and sulfur dioxide (middle panel in Figure 6). Ta.
しかし、二酸化硫黄と酸素が共存すると、図6の下図に示すように、SO4で表面が覆われた状態が熱力学的に安定となり、メタン活性しいてはメタン浄化触媒の作用が失われることがわかった。なおこの硫黄被毒の表面状態生成には、SO2およびSO4の吸着が必要でそれには隣接する2個のPd(3f)と1個のPd(4f)が必要なことが図5上図よりわかる。メタン浄化の触媒作用と硫黄被毒作用に必要な表面Pd原子が異なることを利用して、何らかの方法でメタン浄化活性を維持しつつ硫黄被毒を抑制する触媒を開発することが望まれていた。 However, when sulfur dioxide and oxygen coexist, as shown in the lower part of Figure 6, the state where the surface is covered with SO 4 becomes thermodynamically stable, and when methane becomes active, the action of the methane purification catalyst is lost. I understand. Note that the generation of this sulfur poisoning surface state requires the adsorption of SO 2 and SO 4 , which requires two adjacent Pd(3f) and one Pd(4f), as shown in the upper diagram of Figure 5. I understand more. Taking advantage of the difference in surface Pd atoms required for methane purification catalytic action and sulfur poisoning action, it was hoped to develop a catalyst that would somehow maintain methane purification activity while suppressing sulfur poisoning. .
本発明は、以上のような従来技術の実状に鑑みてなされたもので、メタン浄化活性を損なうことなく、硫黄被毒を抑制することができる排ガス浄化用途に好適な耐硫黄被毒性を有するメタン浄化触媒を提供することを課題とする。 The present invention has been made in view of the actual state of the prior art as described above, and it provides a methane with sulfur poisoning resistance suitable for exhaust gas purification applications that can suppress sulfur poisoning without impairing methane purification activity. Our goal is to provide purification catalysts.
本発明によれば、上記課題を解決するため、下記の発明が提供される。 According to the present invention, the following invention is provided in order to solve the above problems.
〔1〕PdO(101)面の最表面原子に、酸素原子が3配位した原子(3f)と4配位した原子(4f)が存在するPdOにおいて、前記酸素原子が3配位した原子(3f)の少なくとも一部がPd以外の原子Mと置換されていることを特徴とする耐硫黄被毒性を有するメタン浄化触媒。 [1] In PdO, an atom (3f) with three-coordinated oxygen atoms and an atom (4f) with four-coordinated oxygen atoms exist on the outermost surface atoms of the PdO (101) plane. A methane purification catalyst having resistance to sulfur poisoning, characterized in that at least a part of 3f) is replaced with an atom M other than Pd.
〔2〕上記第〔1〕の発明において、M原子が、最表面の金属原子数に対して1/4以上1/2未満の量で、最表面に配置されていることを特徴とする耐硫黄被毒性を有するメタン浄化触媒。
〔3〕上記第〔1〕または〔2〕の発明において、M原子がAuもしくはAgであることを特徴とするメタン浄化触媒。
[2] In the invention [1] above, M atoms are arranged on the outermost surface in an amount of 1/4 or more and less than 1/2 of the number of metal atoms on the outermost surface. Methane purification catalyst with sulfur toxicity.
[3] The methane purification catalyst according to the invention [1] or [2] above, wherein the M atom is Au or Ag.
本発明によれば、上記構成を採用することで、メタン浄化活性を損なうことなく、硫黄被毒を抑制することができる排ガス浄化用途に好適な耐硫黄被毒性を有するメタン浄化触媒を提供することが可能となる。 According to the present invention, there is provided a methane purification catalyst having a sulfur poisoning resistance suitable for exhaust gas purification, which is capable of suppressing sulfur poisoning without impairing methane purification activity by adopting the above configuration. becomes possible.
以下、本発明を実施の形態に基づき詳細に説明する。 Hereinafter, the present invention will be described in detail based on embodiments.
本発明のメタン浄化触媒は、メタン、SO2等の硫黄化合物およびストイキオメトリー以上の酸素を含む被処理ガスを処理対象とする。ここで、硫黄化合物は10ppm程度まで含まれていてもよい。また、ストイキオメトリー以上の酸素とは、被処理ガス中の炭化水素、一酸化炭素などの還元性成分を完全酸化するのに必要な量以上のことをいう。被処理ガスの処理温度は300~500℃程度である。 The methane purification catalyst of the present invention targets a gas to be treated that contains methane, sulfur compounds such as SO 2 , and oxygen above the stoichiometry. Here, the sulfur compound may be contained up to about 10 ppm. In addition, the amount of oxygen exceeding stoichiometry refers to an amount exceeding the amount necessary to completely oxidize reducing components such as hydrocarbons and carbon monoxide in the gas to be treated. The processing temperature of the gas to be processed is approximately 300 to 500°C.
本発明のメタン浄化触媒は、Al2O3、ZrO2、SiO2、CeO2、Y2O3、La2O3等の酸化物担体の1種以上にPdOのPd(3f)の一部をAuで置き換えたAu3f-PdOを担持して構成される。PdOの担持量は、担体に対して重量割合で1~3%程度が好ましい。PdOの担持量が上記範囲であると、適切なメタン浄化活性を得ることができる。 The methane purification catalyst of the present invention contains a part of Pd(3f) of PdO in one or more oxide carriers such as Al 2 O 3 , ZrO 2 , SiO 2 , CeO 2 , Y 2 O 3 , La 2 O 3 and the like. It is composed of supporting Au 3f -PdO with Au replaced with Au. The amount of PdO supported is preferably about 1 to 3% by weight relative to the carrier. When the supported amount of PdO is within the above range, appropriate methane purification activity can be obtained.
メタン浄化活性を維持しつつ硫黄被毒を抑制する触媒を創案するために、本発明者らが前記の非特許文献1で報告した研究を通して得た知見は次の2つである。
In order to create a catalyst that suppresses sulfur poisoning while maintaining methane purification activity, the following two findings were obtained by the present inventors through the research reported in the above-mentioned
条件1.メタン浄化活性には、PdO(101)最表面のPd(3f)原子が必要である。
条件2.硫黄被毒には、隣接する2個のPd(3f)と、それに隣接する1個のPd(4f)が必要である。 Condition 2. Sulfur poisoning requires two adjacent Pd(3f) and one adjacent Pd(4f).
メタンを浄化するメタン浄化活性を維持しつつ硫黄被毒を抑制するには、条件1を満たしつつ、条件2を崩し、かつ安定な表面を形成する必要がある。本発明者らは、これらの知見に基づいて鋭意検討を行い、次の2つの方策について考察した。
In order to suppress sulfur poisoning while maintaining the methane purification activity that purifies methane, it is necessary to satisfy
方策1:PdO(101)最表面のPd(4f)原子を他の元素の原子に置換し、SO2に対して不活性にする。 Strategy 1: Substitute the Pd(4f) atoms on the outermost surface of PdO(101) with atoms of other elements to make it inert to SO 2 .
図7に、置換モデルとその安定性を示す。図7の左上の図に置換を行っていないPdO(101)の最表面の状態を示す。図7の左の真ん中の図はPd(4f)を他の元素Mで置き換えた最表面の状態を示す。図7の左下の図はPd(3f)を他の元素Mで置き換えた最表面の状態を示す。置き換える元素として、M = Cr, Mn, Fe, Co, Ni, Cu, Mo, Tc, Ru, Rh, Ag, W, Re, Os, Ir, Pt, Auについて調べた。図7の右図にエネルギー安定性を示す。縦軸のΔEの絶対値は安定性とは無関係である。図中、○が3f、◇が4fのデータである。3fと4fのエネルギーの大小関係で、ΔEが小さい方が安定である。たとえば、金(Au)の場合、Pd(4f)よりPd(3f)と置換した方が安定である。Pd(4f)と確実に置換できるのはM = Cr, Mn, W, Ir, Ptである。 Figure 7 shows the substitution model and its stability. The upper left diagram in FIG. 7 shows the state of the outermost surface of PdO(101) without substitution. The middle diagram on the left of FIG. 7 shows the state of the outermost surface in which Pd(4f) is replaced with another element M. The lower left diagram in FIG. 7 shows the state of the outermost surface in which Pd(3f) is replaced with another element M. We investigated M = Cr, Mn, Fe, Co, Ni, Cu, Mo, Tc, Ru, Rh, Ag, W, Re, Os, Ir, Pt, and Au as replacement elements. The right diagram in Figure 7 shows energy stability. The absolute value of ΔE on the vertical axis is unrelated to stability. In the figure, ○ is data for 3f and ◇ is data for 4f. Regarding the energy size relationship between 3f and 4f, the smaller ΔE is, the more stable it is. For example, in the case of gold (Au), it is more stable to replace it with Pd(3f) than with Pd(4f). M = Cr, Mn, W, Ir, Pt can be definitely replaced with Pd(4f).
浄化活性と被毒作用を比較するため、Pd(4f)を他の原子Mで置換した場合のCH4とSO2の吸着エネルギーを図8に示す。CH4の吸着エネルギーの絶対値が大きくなり、SO2の吸着エネルギーの絶対値が小さくなるのが候補となる(図中の薄灰色の領域)。銅(Cu)とニッケル(Ni)が、その範囲に入っているが、これらは、Pd(3f)を置換した方が安定なため不適である。この方法では、調査範囲で好適な元素Mはなかった。 In order to compare purification activity and poisoning effect, Figure 8 shows the adsorption energy of CH 4 and SO 2 when Pd(4f) is replaced with another atom M. Candidates are those where the absolute value of adsorption energy for CH 4 becomes large and the absolute value of adsorption energy for SO 2 becomes small (light gray area in the figure). Copper (Cu) and nickel (Ni) fall within this range, but these are unsuitable because they are more stable when replaced with Pd(3f). In this method, there was no suitable element M within the investigation range.
方策2:Pd(3f)原子を部分的に他の元素の原子Mに置換し、隣接するPd(3f)をなくす、若しくは隣接するPd(3f)を減らし、SO2に対する活性を抑制する。 Strategy 2: Partially replace Pd(3f) atoms with atoms M of other elements, eliminate or reduce adjacent Pd(3f), and suppress activity toward SO 2 .
図9に、置換モデル(左図)とそのエネルギー安定性を示す。図9の左上の図はPd(3f)の一部を他の原子Mで置換した最表面の状態を示し、左下の図はPd(4f)の一部を他の原子Mで置換した最表面の状態を示す。置き換える原子Mとして、M = Cr, Mn, Fe, Co, Ni, Cu, Mo, Tc, Ru, Rh, Ag, W, Re, Os, Ir, Pt, Auについて調べた。図9の右図にエネルギー安定性を示す。図7と同様、縦軸のΔEの絶対値は安定性とは無関係である。図中、○が3f、◇が4fのデータである。3fと4fのエネルギーの大小関係で、ΔEが小さい方が安定である。この場合、M = Ni, Cu, Ag, Auの場合がPd(4f)よりPd(3f)と置換した方が安定である。Pd(3f)と置換した場合のCH4とSO2の吸着エネルギーを図10に示す。最も好適な関係にあるのは金(M=Au)の場合であることが分かった。金には劣るがM=Agも若干の効果が期待できる。 Figure 9 shows the substitution model (left figure) and its energy stability. The upper left diagram in Figure 9 shows the top surface state where a part of Pd(3f) is replaced with other atoms M, and the lower left diagram shows the top surface state where a part of Pd(4f) is replaced with another atom M. Indicates the status of As the replacement atom M, M = Cr, Mn, Fe, Co, Ni, Cu, Mo, Tc, Ru, Rh, Ag, W, Re, Os, Ir, Pt, and Au were investigated. The right diagram in Figure 9 shows energy stability. Similar to FIG. 7, the absolute value of ΔE on the vertical axis is unrelated to stability. In the figure, ○ is data for 3f and ◇ is data for 4f. Regarding the energy size relationship between 3f and 4f, the smaller ΔE is, the more stable it is. In this case, when M = Ni, Cu, Ag, Au, substitution with Pd(3f) is more stable than Pd(4f). Figure 10 shows the adsorption energies of CH 4 and SO 2 when replaced with Pd(3f). It was found that the most favorable relationship is in the case of gold (M=Au). M=Ag can also be expected to have some effect, although it is inferior to gold.
図11にもとのPdO(101)表面と、同表面でPd(3f)を一つ置きに金原子に置換した場合のCH4およびSO2の吸着状態を示す。図11において、右図で大きい薄い灰色の球がPd、右図の右側上下の図でSO2が吸着している大きい灰色の球がAu、Pdと結合している小さい濃い灰色の球がPdOのO、右図の右側上下のSO2の中央の小さい薄い灰色の球がSO2のS、右図の右側上下のSO2の小さい濃い灰色の球がSO2のO、右図の左側上下のPd(3f)に吸着しているCH4の中央の小さい濃い灰色の球がC、右図の左側上下のPd(3f)に吸着しているCH4の小さい薄い灰色の球がHである。CH4は、どちらの表面でも同じ形態で吸着しているのに対して、SO2の場合は、OおよびSがPdのトップに向かう形で吸着していた形態が、2つのOが向かうべき隣接するPd(3f)が失われ、Sが金へ、片方のOのみがPdへ吸着する形態に代わっていることが分かる。これが、SO2の吸着エネルギーが下がった原因である。 FIG. 11 shows the adsorption states of CH 4 and SO 2 on the original PdO(101) surface and when every other Pd(3f) on the same surface was replaced with gold atoms. In Figure 11, the large light gray sphere on the right is Pd, the large gray sphere adsorbing SO 2 on the upper and lower right side of the right figure is Au, and the small dark gray sphere bonded to Pd is PdO. The small light gray sphere in the center of SO 2 on the upper and lower right side of the right figure is the S of SO 2 , the small dark gray sphere of SO 2 on the upper and lower right side of the right figure is the O of SO 2 , and the upper and lower left side of the right figure The small dark gray sphere in the center of CH 4 adsorbed on Pd(3f) is C, and the small light gray sphere of CH 4 adsorbed on Pd(3f) on the upper and lower left side of the right figure is H. . CH 4 is adsorbed in the same form on both surfaces, whereas in the case of SO 2 , the adsorption form in which O and S are directed toward the top of Pd is different from the one in which the two O's should be directed. It can be seen that the adjacent Pd(3f) is lost, S is adsorbed to gold, and only one O is adsorbed to Pd. This is the reason why the adsorption energy of SO 2 has decreased.
O2とSO2が同時に存在する場合の安定な表面吸着状態を調査した結果を図12に示す。白抜き星(☆)シンボルは、典型的なメタン浄化実験条件のガス分圧環境を示す:T=400℃:Po_2=0.20 atm, Pso_2=5x10-6atm。Pd(3f)を一つ置きにAuに置換することにより、酸化しにくくなり、O2、SO2、SO4の吸着安定領域が縮小され、典型的な実験分圧では清浄表面が安定であることが分かった。すなわち、Pd(3f)の一部をAuに置換することにより、SO2が酸化したSO4で覆われてしまうことが抑止され、かつ、メタン浄化活性なPd(3f)が残されており、メタンの浄化反応は抑制されない。なお、この場合、Pd(3f)の数は半分になっているが、もともとCH4が吸着し、反応が進んでいる隣のPd(3f)は、吸着メタン同士の相互作用のため浄化活性は失っている。すなわちオリジナルのPdO表面に比べ浄化活性が落ちるものではない。 Figure 12 shows the results of investigating the stable surface adsorption state when O 2 and SO 2 are present simultaneously. The open star (☆) symbol indicates the gas partial pressure environment under typical methane purification experimental conditions: T=400℃: Po_ 2 =0.20 atm, Pso_ 2 =5x10 -6 atm. By substituting every other Pd(3f) with Au, it becomes less susceptible to oxidation, and the stable adsorption region for O 2 , SO 2 , and SO 4 is reduced, making the clean surface stable at typical experimental partial pressures. That's what I found out. That is, by substituting a part of Pd(3f) with Au, SO 2 is prevented from being covered with oxidized SO 4 , and Pd(3f), which is active in methane purification, remains. The methane purification reaction is not suppressed. In this case, the number of Pd(3f) has been halved, but the neighboring Pd(3f), on which CH 4 has originally been adsorbed and the reaction is progressing, has no purification activity due to the interaction between the adsorbed methane. I'm losing it. In other words, the purification activity is not lower than that of the original PdO surface.
残されたPd(3f)における浄化活性を評価した結果を図13に示す。分子状吸着状態(CH4*)からの活性化障壁は0.68eV で、0.02eV高くなっているが、その差は極めて低く、常温で反応が進む状態であることは変わりなく、むしろCH4分子状吸着の吸着エネルギーの絶対値の増加分だけ、反応活性が上がっている。 The results of evaluating the purification activity of the remaining Pd(3f) are shown in FIG. 13. The activation barrier from the molecular adsorption state (CH 4 *) is 0.68 eV, which is 0.02 eV higher, but the difference is extremely small and the reaction is still in a state where the reaction proceeds at room temperature. The reaction activity increases by the amount of increase in the absolute value of the adsorption energy of the .
この系では金は表面偏析する特性をもつため、適量のAuをPdに混ぜて液相還元法等で金属ナノ粒子を作成すれば、ナノ粒子の表面にAuが析出してくる。それを酸化してPdOを作成すると、Auは、Pd(4f)よりは、Pd(3f)と置換する方が安定であるから、自動的にPd(3f)の位置にAuが配置される。最も好適なAu原子の数は表面原子の1/4の量であるが、それ以上でも隣り合わないPd(3f)が残れば硫黄被毒でメタン浄化活性が失活するものではない。そのためAu原子数は表面原子数の1/4以上1/2未満の量が望ましい。 In this system, gold has the property of segregating on the surface, so if a suitable amount of Au is mixed with Pd and metal nanoparticles are created using a liquid phase reduction method, Au will precipitate on the surface of the nanoparticles. When it is oxidized to create PdO, since Au is more stable when substituted with Pd(3f) than with Pd(4f), Au is automatically placed in the position of Pd(3f). The most preferable number of Au atoms is 1/4 of the number of surface atoms, but even if the number is more than that, if non-adjacent Pd(3f) remains, the methane purification activity will not be deactivated due to sulfur poisoning. Therefore, the number of Au atoms is preferably 1/4 or more and less than 1/2 of the number of surface atoms.
例えば、直径3.7nmの金属ナノ粒子の場合、全原子数に対して、6.3%~12.6%のAu原子を混ぜれば良い。原子数比でAu:Pd = 1:15~1:7、重量比で1:8~1:4に相当する。 For example, in the case of metal nanoparticles with a diameter of 3.7 nm, it is sufficient to mix 6.3% to 12.6% of Au atoms based on the total number of atoms. The atomic ratio corresponds to Au:Pd = 1:15 to 1:7, and the weight ratio corresponds to 1:8 to 1:4.
また、メタン浄化触媒は、一般のPdO担持触媒と同様な温度、時間条件で焼成処理を行い使用することができる。 Furthermore, the methane purification catalyst can be used after being subjected to a calcination treatment under the same temperature and time conditions as general PdO supported catalysts.
液相還元法で、AuとPtを原子数比で1:4および1:15で混合しナノ合金を作成しZrO2上に担持した触媒を用いてモデル排ガス(CH4=0.1%, O2=10%, SO2=5ppm, H2O=3%、他He)でメタン浄化活性を実験で検証した。図14に得られたメタン浄化率の温度依存性を示す。比較のためPt、Ir、Ruを同様にZrO2上に担持した触媒の結果を記した。Pt、Ruより、低温からIrと同等の高メタン浄化率を示し、メタン浄化触媒作用がSO2、O2存在下でもあることが示された。 Using a liquid-phase reduction method, nanoalloys were created by mixing Au and Pt in atomic ratios of 1:4 and 1:15, and a model exhaust gas (CH 4 =0.1%, O 2 =10%, SO 2 =5ppm, H 2 O =3%, and other He).The methane purification activity was verified experimentally. FIG. 14 shows the temperature dependence of the obtained methane purification rate. For comparison, the results of catalysts in which Pt, Ir, and Ru were similarly supported on ZrO 2 are shown. Compared with Pt and Ru, it showed a high methane purification rate equivalent to that of Ir at low temperatures, and it was shown that the methane purification catalytic action can be performed even in the presence of SO 2 and O 2 .
Claims (2)
前記原子MがAuおよびAgの何れか一方または双方であることを特徴とする耐硫黄被毒性を有するメタン浄化触媒。 In PdO, an atom (3f) with three coordinated oxygen atoms and an atom (4f) with four coordinated oxygen atoms exist on the outermost surface atom of the PdO (101) plane, and the atom (3f) with three coordinated oxygen atoms exists. At least a portion is substituted with atoms M other than Pd atoms ,
A methane purification catalyst having resistance to sulfur poisoning, characterized in that the atom M is one or both of Au and Ag .
The sulfur-resistant coating according to claim 1, wherein the atoms M are arranged on the outermost surface in an amount of 1/4 or more and less than 1/2 of the number of metal atoms on the outermost surface. A toxic methane purification catalyst.