JP3125712B2 - Method and apparatus for manufacturing seamless metal pipe - Google Patents

Method and apparatus for manufacturing seamless metal pipe

Info

Publication number
JP3125712B2
JP3125712B2 JP09120660A JP12066097A JP3125712B2 JP 3125712 B2 JP3125712 B2 JP 3125712B2 JP 09120660 A JP09120660 A JP 09120660A JP 12066097 A JP12066097 A JP 12066097A JP 3125712 B2 JP3125712 B2 JP 3125712B2
Authority
JP
Japan
Prior art keywords
pipe
roll
gap
diameter
caliber
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Expired - Fee Related
Application number
JP09120660A
Other languages
Japanese (ja)
Other versions
JPH10305305A (en
Inventor
達也 奥井
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Nippon Steel Corp
Original Assignee
Sumitomo Metal Industries Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Sumitomo Metal Industries Ltd filed Critical Sumitomo Metal Industries Ltd
Priority to JP09120660A priority Critical patent/JP3125712B2/en
Publication of JPH10305305A publication Critical patent/JPH10305305A/en
Application granted granted Critical
Publication of JP3125712B2 publication Critical patent/JP3125712B2/en
Anticipated expiration legal-status Critical
Expired - Fee Related legal-status Critical Current

Description

【発明の詳細な説明】DETAILED DESCRIPTION OF THE INVENTION

【0001】[0001]

【産業上の利用分野】本発明は、継目無金属管の製造方
法に係わり、特に同じキャリバーロールを用いて外径の
異なる外径に仕上げることが可能な熱間定径圧延機を用
いた継目無金属管の製造方法に関する。
BACKGROUND OF THE INVENTION 1. Field of the Invention The present invention relates to a method for manufacturing a seamless metal pipe, and more particularly to a seam using a hot constant diameter rolling mill capable of finishing the outer diameters with different diameters using the same caliber roll. The present invention relates to a method for manufacturing a metal-free tube.

【0002】[0002]

【従来の技術】一般的な継目無金属管の製造工程は、ピ
アサーにより穿孔された中空素管をマンドレルミルなど
の延伸圧延機により減肉圧延し、次いでサイザーあるい
はストレッチレデューサーなどの定径圧延機によりその
外径を所定の寸法に定径圧延した後、冷却床で室温にま
で冷却された管を対象に、ロータリーストレートナーな
どの矯正圧延機によって矯正圧延することで管の曲がり
と真円度を矯正する。
2. Description of the Related Art A general process for manufacturing a seamless metal pipe is to reduce the thickness of a hollow shell pierced by a piercer using a stretching rolling machine such as a mandrel mill, and then to reduce the diameter of the hollow pipe to a sizer such as a sizer or a stretch reducer. After the outer diameter of the pipe is rolled to a predetermined size, the pipe is cooled to room temperature by a cooling bed and straightened by a straightening mill such as a rotary straightener to bend and round the pipe. To correct.

【0003】上記の定径圧延機であるサイザーは、同一
平面内に3個のキャリバーロールがパスセンターOの回
りに120°の間隔を隔てて放射状に組み込まれたロー
ルスタンド複数基(通常、5〜28基)を、図1に示す
ように、連設配置することで構成されている。この時、
隣合うロールタンドは、相互の3個のキャリバーロール
配置が図2(a)と図2(b)の関係になるように、パ
スセンターOの回りに60°位相を異ならせて連設され
る。そして、定径圧延時には、仕上げるべき管の外径に
応じて使用すべきロールスタンド数が決定される。
[0003] The sizer, which is the above-mentioned constant diameter rolling mill, has a plurality of roll stands (typically, 5 caliber rolls) in which three caliber rolls are radially incorporated around a pass center O at an interval of 120 ° in the same plane. 1 to 28 units), as shown in FIG. At this time,
Adjacent roll tands are successively provided with a phase difference of 60 ° around the path center O so that the arrangement of the three caliber rolls is in the relationship shown in FIGS. 2A and 2B. Then, at the time of constant diameter rolling, the number of roll stands to be used is determined according to the outer diameter of the pipe to be finished.

【0004】一方、上記の矯正圧延機であるロータリー
ストレートナーは、パスセンターに対して互いに逆向き
に傾斜対向配置された鼓型ロール対または1個の鼓型ロ
ールが組み込まれた複数基のロールスタンドを、例え
ば、図3に示すように、「2−2−2−1」のように連
設配置することで構成されている。そして、矯正圧延時
には、矯正すべき管の外径に応じて隣合うロールスタン
ドのパスセンター高さ(オフセット量)、各ロールスタ
ンドの鼓型ロール対による圧下量(クラッシュ量)およ
び鼓型ロールのパスセンターに対する傾斜角度を適正な
値に設定することによって管の曲がりと真円度を矯正す
るようになっている(例えば、特開昭62−17301
5号公報参照)。
On the other hand, the above-described rotary straightener, which is a straightening mill, comprises a pair of drum-shaped rolls or a plurality of rolls each including a single drum-shaped roll, which are disposed opposite to each other with respect to the pass center. For example, as shown in FIG. 3, the stands are continuously arranged as “2-2-2-1”. At the time of straightening rolling, the height of the pass center of the adjacent roll stand (offset amount), the amount of reduction (crush amount) by the pair of drum-shaped rolls of each roll stand, and the By setting the inclination angle with respect to the path center to an appropriate value, the bending and roundness of the pipe are corrected (for example, Japanese Patent Application Laid-Open No. Sho 62-17301).
No. 5).

【0005】ところで、上記のサイザーによる定径圧延
においては、前述したように、仕上げるべき外径または
肉厚に応じて使用すべきロールスタンド数が決定される
が、このロールスタンド数の調整では対応できない外径
または肉厚に仕上げる場合には、各ロールスタンドのキ
ャリバリーロールを寸法の異なるキャリバーロールに組
み替える必要がある。
[0005] In the above-mentioned constant diameter rolling by the sizer, as described above, the number of roll stands to be used is determined according to the outer diameter or thickness to be finished. When finishing to an outside diameter or wall thickness that cannot be performed, it is necessary to replace the caliber rolls of each roll stand with caliber rolls having different dimensions.

【0006】このため、外径または肉厚が大きく異なる
小口製品の製造時には、頻繁なキャリバーロールの交換
が必要で、そのために多大な時間と労力を費やさなけれ
ばならないので、生産能率が低下する。また、仕上げる
べき外径または肉厚に応じた寸法の異なるキャリバーロ
ールを数多く保有するか、もしくは頻繁にキャリバー寸
法を改削することで対応する必要があるなどの問題があ
った。
[0006] For this reason, when manufacturing small products having greatly different outer diameters or wall thicknesses, frequent replacement of caliber rolls is required, and a great deal of time and labor must be spent for this. As a result, production efficiency is reduced. In addition, there is a problem that a large number of caliber rolls having different dimensions according to the outer diameter or wall thickness to be finished are required, or the caliber dimensions must be frequently reworked to cope with the problem.

【0007】上記の問題を解決する方法としては、例え
ば、特開平7−16616号公報に示される方法があ
る。すなわち、その方法は、真円化のために用いられる
下流側複数基(通常、2〜3基)の仕上げロールスタン
ドを除いた上流側複数基のロールスタンドのキャリバー
ロールのロールギャップを開閉することでキャリバーの
楕円率を変化させ、これによって同じキャリバーロール
を用いて肉厚の異なる同一外径の管に仕上げる方法であ
る。このため、圧延後の管の下式で定義される真円度
は、何ら問題になることもなかった。
As a method for solving the above problem, there is, for example, a method disclosed in JP-A-7-16616. That is, the method is to open and close the roll gap of the caliber roll of the upstream plurality of roll stands excluding the downstream plurality (usually 2 to 3) finishing roll stands used for rounding. In this method, the ellipticity of the caliber is changed, and the same caliber roll is used to finish tubes having different wall thicknesses and the same outer diameter. For this reason, the roundness defined by the following equation of the tube after rolling did not cause any problem.

【0008】真円度(%)={(最大外径−最小外径)
/平均外径}×100(%) しかし、同じキャリバーロールを用いて外径が異なる管
に仕上げる場合には、真円化のために用いられる仕上げ
ロールスタンドのキャリバーロールのロールギャップを
開閉する必要があるが、その開閉量が適切でないと定径
圧延後の管の真円度が劣り、冷却床で室温にまで冷却さ
れた管に矯正圧延を施しても、その真円度が±1%以内
にならないという問題があった。
Roundness (%) = {(maximum outer diameter−minimum outer diameter)
/ Average outer diameter} × 100 (%) However, when finishing pipes with different outer diameters using the same caliber roll, it is necessary to open and close the roll gap of the caliber roll of the finishing roll stand used for rounding. However, if the opening / closing amount is not appropriate, the roundness of the tube after sizing is inferior, and even if the tube cooled to room temperature by the cooling floor is subjected to straightening rolling, the roundness is ± 1%. There was a problem that did not become within.

【0009】[0009]

【発明が解決しようとする課題】本発明は、上記の実状
に鑑みてなされたもので、その課題は、3または4個の
キャリバーロールが同一平面内にギャップ調整自在に組
み込まれたロールスタンド複数基を連設配置してなる熱
間定径圧延機を備え、この定径圧延機のキャリバーロー
ルのギャップを調整することによって種々外径の管に定
径圧延する工程を有する継目無金属管の製造方法におい
て、ロータリーストレートナーによる矯正圧延後の管の
真円度を±1%以内にすることができる継目無金属管の
製造方法と、この方法の実施に用いる継目無金属管の製
造装置を提供することにある。
SUMMARY OF THE INVENTION The present invention has been made in view of the above circumstances, and has as its object to provide a plurality of roll stands in which three or four caliber rolls are incorporated in the same plane so that the gap can be adjusted. A seamless metal pipe having a step of performing constant diameter rolling to pipes having various outer diameters by adjusting a gap of a caliber roll of the constant diameter rolling machine, comprising a hot constant diameter rolling mill having a plurality of bases arranged in series. In the manufacturing method, a method for manufacturing a seamless metal pipe capable of keeping the roundness of a pipe after straightening by a rotary straightener within ± 1%, and a manufacturing apparatus for a seamless metal pipe used for performing the method are described. To provide.

【0010】[0010]

【課題を解決するための手段】本発明者は、上記の課題
を達成すべく、数多くの実験を行った結果、次のことを
知見した。
Means for Solving the Problems The inventor of the present invention has conducted a number of experiments in order to achieve the above object, and has found the following.

【0011】第1の知見は、上記のように構成された定
径圧延機であるサイザーによる圧延の際に、同じキャリ
バーロールのギャップを調整して仕上げるべき平均外径
を、当該キャリバーロールのギャップを基準ギャップに
設定して定径圧延した時に得られる真円管の外径の±2
%の範囲内の平均外径に仕上げる必要があること。
The first finding is that the average outer diameter to be finished by adjusting the gap of the same caliber roll at the time of rolling by the sizer, which is a constant diameter rolling mill configured as described above, is determined by the gap of the caliber roll. ± 2 of the outer diameter of a perfect circular pipe obtained when constant diameter rolling is performed with
It must be finished to an average outer diameter in the range of%.

【0012】第2の知見は、上記範囲内の平均外径に仕
上げられた管を冷却床に送給して室温まで冷却した後に
ロータリーストレートナーによって矯正圧延するのでは
なく、管の温度が500〜650℃である間に矯正圧延
を施した後、管を冷却床に送給して室温まで冷却すれば
よいことである。
The second finding is that, instead of feeding a tube finished to an average outer diameter within the above range to a cooling bed and cooling it to room temperature, and then straightening it by a rotary straightener, the temperature of the tube becomes 500 After performing the straightening while the temperature is 〜650 ° C., the tube may be fed to a cooling floor and cooled to room temperature.

【0013】また、第3の知見は、上記の処理を行うた
めには、その製造装置としてサイザーとロータリースト
レートナーとを連設配置し、ロータリーストレートナー
の下流側に冷却床を配置したレイアウトにする必要があ
ること。
[0013] A third finding is that, in order to perform the above treatment, a layout in which a sizer and a rotary straightener are connected and arranged as a manufacturing apparatus, and a cooling floor is arranged downstream of the rotary straightener. What you need to do.

【0014】さらに、第4の知見は、管温度が500〜
650℃である間にロータリーストレートナーによる矯
正圧延を行う必要のあることから、サイザーとロータリ
ーストレートナーとの間に熱処理炉を介設する場合に
は、オンライン熱処理が可能になるのに加え、省エネが
図れることである。
Further, the fourth finding is that the pipe temperature is 500 to
Since it is necessary to perform straightening rolling using a rotary straightener while the temperature is 650 ° C., when a heat treatment furnace is interposed between the sizer and the rotary straightener, in addition to enabling online heat treatment, energy saving is possible. Is to be achieved.

【0015】上記の知見に基づく本発明の要旨は、下記
(1)および(2)の継目無金属管の製造方法と、下記
(3)および(4)の継目無金属管の製造装置にある。
The gist of the present invention based on the above findings is the following method (1) and (2) for producing a seamless metal pipe and the following (3) and (4) for producing a seamless metal pipe. .

【0016】(1)3または4個のキャリバーロールが
同一平面内にギャップ調整自在に組み込まれたロールス
タンド複数基を連設配置してなる熱間定径圧延機を用
い、この定径圧延機の同じキャリバーロールのギャップ
を調整することによって種々外径の管に定径仕上げ圧延
する工程を有する継目無金属管の製造方法であって、前
記熱間定径圧延機で仕上げる管の平均外径を、当該キャ
リバーロールのギャップを基準ギャップに設定して圧延
した時に得られる真円管の外径の±2%の範囲内に仕上
げ圧延した後、管の温度が500〜650℃である間に
ロータリーストレートナーによって矯正圧延することを
特徴とする継目無金属管の製造方法。
(1) A constant-diameter rolling mill using a hot constant-diameter rolling mill in which a plurality of roll stands in which three or four caliber rolls are incorporated in the same plane so that a gap can be freely adjusted is continuously arranged. A method for producing a seamless metal pipe having a step of performing constant diameter finish rolling to pipes of various outer diameters by adjusting the same caliber roll gap, wherein the average outer diameter of the pipe finished by the hot constant diameter rolling mill After the finish rolling of the caliber roll within the range of ± 2% of the outer diameter of the round pipe obtained by rolling while setting the gap of the caliber roll to the reference gap, while the temperature of the pipe is 500 to 650 ° C. A method for producing a seamless metal pipe, wherein the pipe is straightened by a rotary straightener.

【0017】(2)3または4個のキャリバーロールが
同一平面内にギャップ調整自在に組み込まれたロールス
タンド複数基を連設配置してなる熱間定径圧延機を用
い、この定径圧延機の同じキャリバーロールのギャップ
を調整することによって種々外径の管に定径仕上げ圧延
する工程を有する継目無金属管の製造方法であって、前
記熱間定径圧延機で仕上げる管の平均外径を、当該キャ
リバーロールのギャップを基準ギャップに設定して圧延
した時に得られる真円管の外径の±2%の範囲内に仕上
げ圧延し、次いで定径圧延後の管に所定の熱処理を施し
た後、管の温度が500〜650℃である間にロータリ
ーストレートナーによって矯正圧延することを特徴とす
る継目無金属管の製造方法。
(2) A fixed diameter rolling mill using a hot fixed diameter rolling mill in which a plurality of roll stands in which three or four caliber rolls are incorporated in the same plane so that a gap can be freely adjusted is continuously arranged. A method for producing a seamless metal pipe having a step of performing constant diameter finish rolling to pipes of various outer diameters by adjusting the same caliber roll gap, wherein the average outer diameter of the pipe finished by the hot constant diameter rolling mill Is finished rolled within the range of ± 2% of the outer diameter of the round pipe obtained when the caliber roll gap is set to the reference gap and then subjected to a predetermined heat treatment on the pipe after the constant diameter rolling. And then straightening and rolling by a rotary straightener while the temperature of the tube is 500 to 650 ° C.

【0018】(3)上記(1)に記載の継目無金属管の
製造方法に用いる製造装置であって、3または4個のキ
ャリバーロールが同一平面内にギャップ調整自在に組み
込まれたロールスタンド複数基を連設配置してなる熱間
定径圧延機とロータリーストレートナーとが連続配置さ
れていることを特徴とする継目無金属管の製造装置。
(3) A manufacturing apparatus used in the method for manufacturing a seamless metal pipe according to the above (1), wherein a plurality of roll stands in which three or four caliber rolls are incorporated in the same plane so that a gap can be adjusted. An apparatus for producing a seamless metal pipe, wherein a hot constant-diameter rolling mill in which a plurality of bases are continuously arranged and a rotary straightener are continuously arranged.

【0019】(4)上記(2)に記載の継目無金属管の
製造方法に用いる製造装置であって、3または4個のキ
ャリバーロールが同一平面内にギャップ調整自在に組み
込まれたロールスタンド複数基を連設配置してなる熱間
定径圧延機とロータリーストレートナーとが熱処理炉を
介して連続配置されていることを特徴とする継目無金属
管の製造装置。
(4) A manufacturing apparatus used in the method for manufacturing a seamless metal pipe according to the above (2), wherein a plurality of roll stands in which three or four caliber rolls are incorporated in the same plane so that a gap can be freely adjusted. An apparatus for producing a seamless metal pipe, characterized in that a hot constant diameter rolling mill having a plurality of bases and a rotary straightener are continuously arranged via a heat treatment furnace.

【0020】[0020]

【発明の実施の形態】BEST MODE FOR CARRYING OUT THE INVENTION

《製造方法について》本発明に係わる製造方法では、前
述したように、同じキャリバーロールのギャップを調整
して仕上げるべき管の平均外径を、当該キャリバーロー
ルのギャップを基準ギャップに設定して定径圧延した時
に得られる真円管の外径の±2%の範囲内に仕上げる必
要がある。これは、その仕上げ平均外径が真円管の外径
の±2%を超えると、定径圧延後の管の真円度が悪くな
りすぎ、その後に施すロータリーストレートナーによる
矯正圧延によっても所望の真円度を確保することができ
なくなるからである。
<< Manufacturing Method >> In the manufacturing method according to the present invention, as described above, the same outer diameter of the pipe to be finished by adjusting the gap of the caliber roll is set to the constant diameter by setting the gap of the caliber roll to the reference gap. It is necessary to finish within the range of ± 2% of the outer diameter of the round pipe obtained by rolling. This is because if the average finish outer diameter exceeds ± 2% of the outer diameter of the perfect circular pipe, the roundness of the pipe after the constant diameter rolling becomes too poor, and it is also desired by straightening rolling by a rotary straightener applied thereafter. This is because the roundness cannot be ensured.

【0021】ここで、サイザーを構成する各ロールスタ
ンドのキャリバーロールのギャップ調整は、真円化のた
めに用いられる仕上げロールスタンド(通常、2〜3
基)のキャリバーロールのみを対象に行えば十分である
が、全てのロールスタンドのキャリバーロールを対象に
行ってもよい。
Here, the gap adjustment of the caliber rolls of each roll stand constituting the sizer is performed by using a finishing roll stand (usually 2 to 3) used for rounding.
It is sufficient to perform only the caliber rolls of (base), but it may be performed on the caliber rolls of all roll stands.

【0022】なお、真円化のために用いられる仕上げロ
ールスタンドは、仕上げるべき管外径が大きくなるのに
従って上流側のロールスタンドに順次移行される。そし
て、当該ロールスタンドのうちの少なくとも最下流に位
置するロールスタンドのキャリバーロールが基準ギャッ
プ時に真円キャリバーのキャリバーロールに交換され、
これより下流側に位置するロールスタンドには、例えば
搬送ローラなどが組み込まれる。
The finishing roll stand used for rounding is sequentially transferred to the upstream roll stand as the outer diameter of the pipe to be finished increases. Then, the caliber roll of at least the most downstream roll stand among the roll stands is replaced with a caliber roll of a perfect circular caliber at the time of the reference gap,
For example, a transport roller or the like is incorporated in the roll stand located downstream of the roll stand.

【0023】一方、サイザーによる定径圧延後の管また
はその後サイザーとロータリーストレートナーとの間に
配置された熱処理炉によって所定のオンライン熱処理が
施された管を対象に、その温度が500〜650℃であ
る間に矯正圧延を終了する必要がある。これは、管の温
度が500℃未満になってから矯正圧延してもその矯正
効果が小さく、所望の真円度が得られないためである。
逆に、管の温度が650℃を超える温度域で矯正圧延を
終了すると、矯正圧延後に送られる冷却床で管が変形し
て楕円化し、所望の真円度が確保できなくなるからであ
る。
On the other hand, the temperature of the pipe after the fixed diameter rolling by the sizer or the pipe which has been subjected to a predetermined on-line heat treatment by a heat treatment furnace disposed between the sizer and the rotary straightener is 500 to 650 ° C. , It is necessary to end the straightening rolling. This is because even if straightening rolling is performed after the temperature of the tube is lower than 500 ° C., the straightening effect is small and desired roundness cannot be obtained.
Conversely, when the straightening is finished in a temperature range where the temperature of the tube exceeds 650 ° C., the tube is deformed into an ellipse on the cooling floor sent after the straightening and the desired roundness cannot be secured.

【0024】ここで、管の温度以外のロータリーストレ
ートナーによる矯正圧延条件は特に制限されず、通常の
条件、例えば下記の条件で行えば十分である。
Here, the conditions of the straightening and rolling by the rotary straightener other than the temperature of the tube are not particularly limited, and it is sufficient to carry out under normal conditions, for example, the following conditions.

【0025】オフセット量:1〜15mm、 クラッシュ量:0〜10mm、 鼓型ロールの傾斜角度:25〜35°。Offset amount: 1 to 15 mm, Crash amount: 0 to 10 mm, Tilt angle of drum roll: 25 to 35 °.

【0026】なお、本発明における定径圧延機であるサ
イザーは、ストレッチレデューサーやエキストラクター
サイザーと称されるものであってもよい。さらに、キャ
リバーロールの数は3個に限らず、4個であってもよ
い。
The sizer which is a constant diameter rolling mill in the present invention may be a stretch reducer or an extractor sizer. Further, the number of caliber rolls is not limited to three, but may be four.

【0027】《製造装置について》本発明に係わる製造
装置は、図4に示すように、2通りある。その1つは、
図4の(a)に示すように、上記のサイザーとロータリ
ーストレートナーとを直接連設配置したレイアウトの装
置と、図4の(b)に示すように、上記のサイザーとロ
ータリーストレートナーとを熱処理炉を介して連設配置
したレイアウトの装置である。
<< Production Apparatus >> As shown in FIG. 4, there are two types of production apparatus according to the present invention. One of them is
As shown in FIG. 4 (a), an apparatus having a layout in which the above-mentioned sizer and rotary straightener are directly connected and arranged, and as shown in FIG. 4 (b), the above-mentioned sizer and rotary straightener This is a layout device that is continuously arranged via a heat treatment furnace.

【0028】上記のようなレイアウト配置する時、ロー
タリーストレートナーは、図4(a)の場合にはサイザ
ー、図4(b)の場合には熱処理炉との間隔を余り小さ
くしたり大ききし過ぎると、上記の温度域での矯正圧延
が困難になるので、その設置位置は上記の管温度が得ら
れる距離を隔てるか、もしくは冷却床を介在させて設け
るのが最も好ましい。しかし、実際の工場設計に当たっ
ては敷地形状やその他の諸事情によって必要な離間距離
の確保や冷却床を介在させることができず、その間隔が
必要以上に短くなったり長くなる場合があるが、この場
合にはサイザーまたは熱処理炉の出側に温度計並びに適
宜な加熱装置や冷却装置を配置し、温度計による管の測
温結果に基づいて、加熱装置や冷却装置を作動させてロ
ータリーストレートナーに送給される管の温度を上記の
温度範囲になるように調整するようにするればよいこと
はいうまでもない。
When the layout is arranged as described above, the rotary straightener is provided with a sizer in the case of FIG. 4 (a), and a space between the rotary straightener and the heat treatment furnace in the case of FIG. If it is too long, it is difficult to perform straightening rolling in the above-mentioned temperature range. Therefore, it is most preferable that the installation position is provided at a distance from which the above-mentioned tube temperature can be obtained or with a cooling floor interposed. However, in the actual factory design, it is not possible to secure the required separation distance or intervene the cooling floor due to the site shape and other circumstances, and the spacing may be shorter or longer than necessary. In this case, a thermometer and a suitable heating device or cooling device are arranged on the outlet side of the sizer or heat treatment furnace, and the heating device or cooling device is operated based on the temperature measurement result of the tube by the thermometer to the rotary straightener. It goes without saying that the temperature of the pipe to be fed may be adjusted to be within the above-mentioned temperature range.

【0029】[0029]

【実施例】本発明の効果を立証すべく、3個のキャリバ
ーロールを組み込んだロールスタンド15基を連設配置
したもので、図5に示すように、基準ギャップ時におけ
るキャリバー寸法AおよびBが表1に示す寸法のキャリ
バーロールを各ロールスタンドに組み込んだサイザー
と、2−2−2−1型のロータリーストレートナーを準
備し、次の実験を行った。
EXAMPLE In order to prove the effect of the present invention, fifteen roll stands incorporating three caliber rolls are arranged in a row, and as shown in FIG. A sizer in which caliber rolls having the dimensions shown in Table 1 were incorporated in each roll stand and a 2-2-2-2-1 type rotary straightener were prepared, and the following experiment was performed.

【0030】[0030]

【表1】 [Table 1]

【0031】実験は、上記のサイザーで外径160m
m、肉厚7mmの炭素鋼製素管を外径80mm、肉厚8
mmに定径圧延するに当たり、スタンドNo. 15のキャ
リバーロールのギャップを種々変え、定径圧延後の管の
平均外径を、基準ギャップ時の真円外径の−2.5〜+
2.5%の範囲内の8種類に圧延した。
The experiment was conducted using the above sizer with an outer diameter of 160 m.
m, a 7 mm-thick carbon steel tube with an outer diameter of 80 mm and a thickness of 8
In the case of constant diameter rolling to a diameter of mm, the gap of the caliber roll of stand No. 15 is variously changed, and the average outer diameter of the tube after the constant diameter rolling is -2.5 to + of the true circle outer diameter at the reference gap.
It was rolled to eight types within a range of 2.5%.

【0032】なお、この圧延時、No. 15のキャリバー
ロールにかかる負荷がその基準ギャップ時に比べて極端
に大きくならないようにするために、スタンドNo. 14
のギャップをNo. 15の1/2、No. 13のギャップを
No. 15の1/4の量で同時に調整した。
In order to prevent the load applied to the caliber roll of No. 15 during the rolling from becoming extremely large as compared with the reference gap, the stand No. 14 is used.
Gap of No. 15 and No. 13 gap
No. 15 was adjusted at the same time in an amount of 1/4.

【0033】次いで、得られた8種類の管を対象に、管
の温度を450〜700℃の間で種々変え、上記のロー
タリーストレートナーで下記条件のもとに矯正圧延を行
った後、管を冷却床に送給して0.1rpmで回転させ
つつ室温にまで放冷した。
Next, for the obtained eight kinds of pipes, the pipe temperature was variously changed between 450 to 700 ° C., and the above-mentioned rotary straightener was subjected to straightening rolling under the following conditions, and then the pipe was formed. Was fed to a cooling bed and allowed to cool to room temperature while rotating at 0.1 rpm.

【0034】オフセット量:5mm、 クラッシュ量:2mm、 鼓型ロールの傾斜角度:30°。The amount of offset: 5 mm, the amount of crush: 2 mm, the inclination angle of the drum roll: 30 °.

【0035】そして、冷却後の管を対象に、前述の式で
定義される真円度を調べた。その結果を、サイザーによ
る仕上げ平均外径とその時の真円度、および矯正圧延時
の管温度と併せて表2に示した。
The roundness defined by the above equation was examined for the cooled pipe. The results are shown in Table 2 together with the average finish outer diameter by a sizer, the roundness at that time, and the tube temperature during straightening rolling.

【0036】[0036]

【表2】 [Table 2]

【0037】表2に示す結果から明らかなように、本発
明の方法に従って製造された管の真円度は1%以下で、
所望の真円度を有する製品管が得られている。
As is evident from the results shown in Table 2, the roundness of the tube manufactured according to the method of the present invention is less than 1%,
A product tube having the desired roundness has been obtained.

【0038】これに対し、ロータリーストレートナーに
よる矯正時の管温度が700℃の場合には、管温度が高
いために冷却床で管が変形し、1%以下の真円度を有す
る製品管は得られなかった。また、矯正時の管温度が5
00℃以下の450℃では、サイザーによる仕上げ平均
外径が真円管の外径の±2.5%の場合には、1%以下
の真円度を有する製品管は得られなかった。
On the other hand, when the pipe temperature at the time of straightening by the rotary straightener is 700 ° C., the pipe is deformed on the cooling floor due to the high pipe temperature, and the product pipe having a roundness of 1% or less cannot be obtained. Could not be obtained. In addition, the pipe temperature at the time of straightening is 5
At 450 ° C. below 00 ° C., when the average finish outer diameter by the sizer was ± 2.5% of the outer diameter of the round pipe, a product pipe having a roundness of 1% or less could not be obtained.

【0039】[0039]

【発明の効果】本発明によれば、サイザーの1種類のロ
ールで異なる外径の管を定径圧延する場合にも、真円度
1%以下の製品管を確実に得ることができる。
According to the present invention, a product pipe having a roundness of 1% or less can be reliably obtained even when pipes having different outer diameters are rolled with a single type of roll of a sizer.

【図面の簡単な説明】[Brief description of the drawings]

【図1】3ロール式サイザーの全体構成を示す模式的側
面図である。
FIG. 1 is a schematic side view showing the entire configuration of a three-roll sizer.

【図2】3ロール式サイザーのキャリバーロールの配置
を示す模式的正面図である。
FIG. 2 is a schematic front view showing the arrangement of caliber rolls of a three-roll sizer.

【図3】2−2−2−1型のロータリーストレートナー
の全体構成を示す模式的側面図である。
FIG. 3 is a schematic side view showing the entire configuration of a 2-2-2-1-1 type rotary straightener.

【図4】本発明に係わる継目無金属管の製造装置を示す
図である。
FIG. 4 is a view showing an apparatus for manufacturing a seamless metal pipe according to the present invention.

【図5】実験に用いたキャリバーロールのキャリバー形
状と寸法を示す模式図である。
FIG. 5 is a schematic diagram showing a caliber shape and dimensions of a caliber roll used in an experiment.

【符号の説明】[Explanation of symbols]

1:ロールスタンド、 2:キャリバーロール、 3:金属管、 4:鼓型ロール、 O:パスセンター。 1: Roll stand, 2: Caliber roll, 3: Metal tube, 4: Hour roll, O: Pass center.

Claims (4)

(57)【特許請求の範囲】(57) [Claims] 【請求項1】3または4個のキャリバーロールが同一平
面内にギャップ調整自在に組み込まれたロールスタンド
複数基を連設配置してなる熱間定径圧延機を用い、この
定径圧延機の同じキャリバーロールのギャップを調整す
ることによって種々外径の管に定径仕上げ圧延する工程
を有する継目無金属管の製造方法であって、前記熱間定
径圧延機で仕上げる管の平均外径を、当該キャリバーロ
ールのギャップを基準ギャップに設定して圧延した時に
得られる真円管の外径の±2%の範囲内に仕上げ圧延し
た後、管の温度が500〜650℃である間にロータリ
ーストレートナーによって矯正圧延することを特徴とす
る継目無金属管の製造方法。
1. A hot constant-diameter rolling mill comprising a plurality of roll stands in which three or four caliber rolls are incorporated in the same plane so that a gap can be freely adjusted. A method for producing a seamless metal pipe having a step of performing constant-diameter finish rolling to pipes of various outer diameters by adjusting the gap of the same caliber roll, wherein the average outer diameter of the pipe finished by the hot constant-diameter rolling mill is After the calender roll is set to the reference gap and rolled in a range of ± 2% of the outer diameter of the round pipe obtained when rolling is performed, the rotary is performed while the temperature of the pipe is 500 to 650 ° C. A method for producing a seamless metal pipe, comprising straightening and rolling with a straightener.
【請求項2】3または4個のキャリバーロールが同一平
面内にギャップ調整自在に組み込まれたロールスタンド
複数基を連設配置してなる熱間定径圧延機を用い、この
定径圧延機の同じキャリバーロールのギャップを調整す
ることによって種々外径の管に定径仕上げ圧延する工程
を有する継目無金属管の製造方法であって、前記熱間定
径圧延機で仕上げる管の平均外径を、当該キャリバーロ
ールのギャップを基準ギャップに設定して圧延した時に
得られる真円管の外径の±2%の範囲内に仕上げ圧延
し、次いで定径圧延後の管に所定の熱処理を施した後、
管の温度が500〜650℃である間にロータリースト
レートナーによって矯正圧延することを特徴とする継目
無金属管の製造方法。
2. A hot constant-diameter rolling mill comprising a plurality of roll stands in which three or four caliber rolls are incorporated in the same plane so that a gap can be freely adjusted. A method for producing a seamless metal pipe having a step of performing constant-diameter finish rolling to pipes of various outer diameters by adjusting the gap of the same caliber roll, wherein the average outer diameter of the pipe finished by the hot constant-diameter rolling mill is The caliber roll gap was set to a reference gap, the finish rolled to a range of ± 2% of the outer diameter of the round pipe obtained when rolling was performed, and then the pipe after the fixed diameter rolling was subjected to a predetermined heat treatment. rear,
A method for producing a seamless metal pipe, wherein the pipe is straightened by a rotary straightener while the temperature of the pipe is 500 to 650 ° C.
【請求項3】請求項1に記載の継目無金属管の製造方法
に用いる製造装置であって、3または4個のキャリバー
ロールが同一平面内にギャップ調整自在に組み込まれた
ロールスタンド複数基を連設配置してなる熱間定径圧延
機とロータリーストレートナーとが連続配置されている
ことを特徴とする継目無金属管の製造装置。
3. A manufacturing apparatus for use in the method for manufacturing a seamless metal pipe according to claim 1, comprising a plurality of roll stands in which three or four caliber rolls are incorporated in the same plane so that a gap can be adjusted. An apparatus for manufacturing a seamless metal pipe, wherein a hot constant diameter rolling mill and a rotary straightener, which are continuously arranged, are continuously arranged.
【請求項4】請求項2に記載の継目無金属管の製造方法
に用いる製造装置であって、3または4個のキャリバー
ロールが同一平面内にギャップ調整自在に組み込まれた
ロールスタンド複数基を連設配置してなる熱間定径圧延
機とロータリーストレートナーとが熱処理炉を介して連
続配置されていることを特徴とする継目無金属管の製造
装置。
4. A manufacturing apparatus for use in a method for manufacturing a seamless metal pipe according to claim 2, comprising a plurality of roll stands in which three or four caliber rolls are incorporated in the same plane so that a gap can be adjusted. An apparatus for manufacturing a seamless metal pipe, wherein a hot constant diameter rolling mill and a rotary straightener, which are continuously arranged, are continuously arranged via a heat treatment furnace.
JP09120660A 1997-05-12 1997-05-12 Method and apparatus for manufacturing seamless metal pipe Expired - Fee Related JP3125712B2 (en)