JP2015103573A - Thermosetting die bond film, die bond film with dicing sheet and method for manufacturing semiconductor device - Google Patents

Thermosetting die bond film, die bond film with dicing sheet and method for manufacturing semiconductor device Download PDF

Info

Publication number
JP2015103573A
JP2015103573A JP2013241284A JP2013241284A JP2015103573A JP 2015103573 A JP2015103573 A JP 2015103573A JP 2013241284 A JP2013241284 A JP 2013241284A JP 2013241284 A JP2013241284 A JP 2013241284A JP 2015103573 A JP2015103573 A JP 2015103573A
Authority
JP
Japan
Prior art keywords
die
thermosetting
bonding
film
die bond
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
JP2013241284A
Other languages
Japanese (ja)
Inventor
木村 雄大
Takehiro Kimura
雄大 木村
三隅 貞仁
Sadahito Misumi
貞仁 三隅
謙司 大西
Kenji Onishi
謙司 大西
悠樹 菅生
Yuki Sugao
悠樹 菅生
雄一郎 宍戸
Yuichiro Shishido
雄一郎 宍戸
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Nitto Denko Corp
Original Assignee
Nitto Denko Corp
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Nitto Denko Corp filed Critical Nitto Denko Corp
Priority to JP2013241284A priority Critical patent/JP2015103573A/en
Priority to KR1020140067849A priority patent/KR20140142675A/en
Priority to CN201410245350.4A priority patent/CN104212369A/en
Priority to TW103119363A priority patent/TW201506116A/en
Publication of JP2015103573A publication Critical patent/JP2015103573A/en
Pending legal-status Critical Current

Abstract

PROBLEM TO BE SOLVED: To provide a thermosetting die bond film having a high thermal conductivity, and arranged to be able to sufficiently follow the unevenness of an object to adhere to when being caused to adhere to the object to adhere to.SOLUTION: A thermosetting die bond film has a post-heat curing thermal conductivity of 1 W/m K or more, and comprises thermally conductive particles having a thermal conductivity of 12 W/m K or more and accounting for 75 wt.% or more to the total weight of the thermosetting die bond film, of which the melt viscosity measured at 130°C with a shear rate of 50(1/second) is 200 Pa s or less.

Description

本発明は、熱硬化型ダイボンドフィルム、ダイシングシート付きダイボンドフィルム、及び、半導体装置の製造方法に関する。   The present invention relates to a thermosetting die bond film, a die bond film with a dicing sheet, and a method for manufacturing a semiconductor device.

近年、半導体装置のデータ処理の高速化が進むにつれて、半導体チップからの発熱量が多くなり、放熱性を持たせた半導体装置の設計の重要性が増している。熱は、半導体装置そのものに対してはもちろん、それを組み込んだ電子機器本体にもさまざまな悪影響を及ぼす。放熱のためのパッケージ対策としては様々な方法が考えられるが、もっとも重要なのがプリント基板やリードフレームなどの基板を介しての放熱である。   In recent years, as the speed of data processing of a semiconductor device increases, the amount of heat generated from a semiconductor chip increases, and the importance of designing a semiconductor device with heat dissipation has increased. Heat affects various adverse effects not only on the semiconductor device itself but also on the electronic device body in which it is incorporated. Various methods can be considered as a package countermeasure for heat dissipation, but the most important is heat dissipation via a substrate such as a printed circuit board or a lead frame.

そこで従来、基板と半導体チップの接着には高熱伝導性を有する接着剤が使用される場合がある。従来この接着剤としては、接着剤の中でも比較的熱伝導率の高い銀ペーストが使用されている。   Therefore, conventionally, an adhesive having high thermal conductivity may be used for bonding the substrate and the semiconductor chip. Conventionally, a silver paste having a relatively high thermal conductivity is used as the adhesive.

しかしながら、近年、スマートフォンやタブレットPCが普及し、高性能化することで、半導体装置の軽薄、短小化が進むにつれて銀ペーストでは半導体装置の組み立てが困難な状況が出てきている。   However, in recent years, with the spread of smartphones and tablet PCs and higher performance, it has become difficult to assemble semiconductor devices with silver paste as the semiconductor devices become lighter and thinner.

具体的には、スマートフォンやタブレットPCの用途にはチップ面積が小さく、薄い半導体チップを用いたパッケージが用いられる。しかしながら、このような半導体チップをペースト状の接着剤で接着しようとすると、半導体チップが薄いために半導体チップが割れてしまったり、半導体チップの回路面に接着剤が回り込んだり、半導体チップに傾きが発生するなど様々な製造上の問題が発生する。また、ペースト状の接着剤は接着させて硬化させるプロセス中でボイドを発生し易い。そのため、半導体チップと基板との間に発生したボイドが放熱の妨げになり、設計通りの熱伝導性(放熱性)を発現できないなどの不良の原因になる。   Specifically, a package using a thin semiconductor chip with a small chip area is used for a smartphone or a tablet PC. However, if such a semiconductor chip is to be bonded with a paste-like adhesive, the semiconductor chip is cracked because the semiconductor chip is thin, the adhesive wraps around the circuit surface of the semiconductor chip, or the semiconductor chip is inclined. Various manufacturing problems occur, such as In addition, a paste-like adhesive tends to generate voids in the process of bonding and curing. For this reason, voids generated between the semiconductor chip and the substrate hinder heat dissipation, and cause defects such as inability to exhibit the designed thermal conductivity (heat dissipation).

一方、従来、シート状のダイボンドフィルムが知られている(例えば、特許文献1参照)。このようなダイボンドフィルムを使用すれば、チップの割れ、接着剤の回り込み、チップの傾きは抑制することができる。しかしながら、従来のダイボンドフィルムは、銀ペーストに比べて熱伝導性が低い点で改良の余地がある。   On the other hand, conventionally, a sheet-like die bond film is known (see, for example, Patent Document 1). If such a die-bonding film is used, chip cracking, adhesive wraparound, and chip tilt can be suppressed. However, the conventional die bond film has room for improvement in that the thermal conductivity is lower than that of the silver paste.

特開2008−218571号公報JP 2008-218571 A

ダイボンドフィルムを高熱伝導性にするには、例えば、高熱伝導性の熱伝導性粒子を高充填に配合する必要がある。しかしながら、熱伝導性粒子を高充填にすることで各種特性においてデメリットが生じる場合がある。すなわち、半導体チップはプリント配線基板など、ある程度表面凹凸の大きいものに貼り合わせて使用されることが多いが、ダイボンドフィルムに熱伝導性粒子を高充填にした状態では、熱伝導性粒子と樹脂の相互作用によってダイボンドフィルムの粘度が高くなることで流動性が低下し、プリント配線基板などの基板の凹凸に十分に追従出来ないという問題が起こる。   In order to make the die-bonding film highly conductive, for example, it is necessary to mix highly heat-conductive particles with high filling. However, there may be a demerit in various characteristics by making the heat conductive particles highly filled. That is, the semiconductor chip is often used by being bonded to a printed wiring board or the like having a certain degree of surface irregularity, but in a state where the thermally conductive particles are highly filled in the die bond film, the thermally conductive particles and the resin are As the viscosity of the die bond film is increased by the interaction, the fluidity is lowered, and there is a problem that the unevenness of the substrate such as a printed wiring board cannot be sufficiently followed.

樹脂を含有するダイボンドフィルムは、通常、せん断応力を加えると粘度が低下する。特に、高速(例えば、ずり速度20〜100(1/秒)程度)でせん断応力を加えると、大きく粘度が低下する。そこで、ダイボンドフィルムを基板に貼り付ける際に、圧力を加えることにより高速せん断応力を生じさせて、粘度を低下させ、基板の凹凸に追従させる方法がある。しかしながら、ダイボンドフィルムに熱伝導性粒子を高充填にした状態では、圧力を加えてせん断応力を生じさせても、粘度が充分に低下せず、ダイボンドフィルムが基板の凹凸に充分追従できない場合があるといった問題がある。   A die bond film containing a resin usually decreases in viscosity when a shear stress is applied. In particular, when shear stress is applied at a high speed (for example, a shear rate of about 20 to 100 (1 / second)), the viscosity is greatly reduced. Thus, there is a method in which when applying the die bond film to the substrate, a high-speed shear stress is generated by applying pressure to reduce the viscosity and follow the unevenness of the substrate. However, in a state where the thermally conductive particles are highly filled in the die bond film, even if pressure is applied to cause shear stress, the viscosity does not sufficiently decrease, and the die bond film may not sufficiently follow the unevenness of the substrate. There is a problem.

そして、ダイボンドフィルムが基板の凹凸に追従出来ない場合、ダイボンドフィルムと基板との間にボイドが生じる。ダイボンドフィルムと基板との間にボイドがあると、前述したように放熱性が低下する問題が起こる他、信頼性が低下し、リフロー工程で被着体との剥離が生じるなどの問題も起こり得るといった問題がある。   And when a die-bonding film cannot follow the unevenness | corrugation of a board | substrate, a void arises between a die-bonding film and a board | substrate. If there is a void between the die-bonding film and the substrate, there will be a problem that the heat dissipation is reduced as described above, and there is a possibility that the reliability is lowered and peeling from the adherend occurs in the reflow process. There is a problem.

本発明は前記問題点に鑑みなされたものであり、その目的は、熱伝導性が高く、且つ、被着体に貼り付ける際に被着体の凹凸に十分に追従することができる熱硬化型ダイボンドフィルム、当該熱硬化型ダイボンドフィルムを用いたダイシングシート付きダイボンドフィルム、及び、当該ダイシングシート付きダイボンドフィルムを用いた半導体装置の製造方法を提供することにある。   The present invention has been made in view of the above problems, and its purpose is a thermosetting type that has high thermal conductivity and can sufficiently follow the unevenness of the adherend when being attached to the adherend. A die bond film, a die bond film with a dicing sheet using the thermosetting die bond film, and a method for manufacturing a semiconductor device using the die bond film with the dicing sheet are provided.

本願発明者等は、前記従来の問題点を解決すべく、熱硬化型ダイボンドフィルムについて検討した。その結果、下記の構成を採用することにより、熱伝導性を高くし、且つ、被着体に貼り付ける際に被着体の凹凸に十分に追従することができることを見出し、本発明を完成させるに至った。   The inventors of the present application have studied a thermosetting die-bonding film in order to solve the conventional problems. As a result, by adopting the following configuration, it is found that the thermal conductivity can be increased and the unevenness of the adherend can be sufficiently followed when being attached to the adherend, thereby completing the present invention. It came to.

すなわち、本発明に係る熱硬化型ダイボンドフィルムは、
熱硬化後の熱伝導率が1W/m・K以上であり、
熱伝導率が12W/m・K以上の熱伝導性粒子を、熱硬化型ダイボンドフィルム全体に対して75重量%以上含有しており、
130℃において、ずり速度50(1/秒)で測定される溶融粘度が200Pa・s以下であることを特徴とする。
That is, the thermosetting die bond film according to the present invention is
The thermal conductivity after thermosetting is 1 W / m · K or more,
Containing 75% by weight or more of thermally conductive particles having a thermal conductivity of 12 W / m · K or more with respect to the entire thermosetting die-bonding film;
The melt viscosity measured at a shear rate of 50 (1 / second) at 130 ° C. is 200 Pa · s or less.

前記構成によれば、熱伝導率が12W/m・K以上の熱伝導性粒子を、熱硬化型ダイボンドフィルム全体に対して75重量%以上含有しており、熱硬化後の熱伝導率が1W/m・K以上であるため、当該熱硬化型ダイボンドフィルムを用いて製造される半導体装置は、放熱性に優れる。
また、130℃において、ずり速度50(1/秒)で測定される溶融粘度、すなわち、130℃における高速せん断時の溶融粘度が200Pa・s以下であるため、熱硬化型ダイボンドフィルムを被着体に貼り付ける際の圧力により、熱硬化型ダイボンドフィルムの粘度が低下する。従って、プリント配線基板などの被着体の凹凸に十分に追従でき、ボイドの発生を抑制することができる。
According to the said structure, the heat conductivity of 12 W / m * K or more is contained 75weight% or more with respect to the whole thermosetting die-bonding film, and the heat conductivity after thermosetting is 1W. Since it is / m · K or more, the semiconductor device manufactured using the thermosetting die-bonding film is excellent in heat dissipation.
Further, since the melt viscosity measured at a shear rate of 50 (1 / second) at 130 ° C., that is, the melt viscosity at high-speed shear at 130 ° C. is 200 Pa · s or less, the thermosetting die bond film is attached to the adherend. The viscosity of the thermosetting die-bonding film decreases due to the pressure applied to the film. Accordingly, it is possible to sufficiently follow the unevenness of the adherend such as a printed wiring board and to suppress the generation of voids.

前記構成において、前記熱伝導性粒子の平均粒径は、1μm以上10μm以下であることが好ましい。   The said structure WHEREIN: It is preferable that the average particle diameter of the said heat conductive particle is 1 micrometer or more and 10 micrometers or less.

前記熱伝導性粒子の平均粒径を1μm以上とすることにより、熱硬化型ダイボンドフィルムの被着体への濡れ性を確保して良好な接着性を発揮させることができる。また、前記熱伝導性粒子の平均粒径を10μm以下とすることにより、熱伝導性粒子の添加による熱伝導性の向上効果をより良好なものとすることができる。また、前記熱伝導性粒子の平均粒径を10μm以下とすることにより、熱硬化型ダイボンドフィルムの厚さを薄くすることができ、ひいては半導体チップを高積層化することができると共に、熱硬化型ダイボンドフィルムから熱伝導性粒子が突き出すことによるチップクラックの発生を防止することができる。   By setting the average particle size of the heat conductive particles to 1 μm or more, it is possible to ensure wettability to the adherend of the thermosetting die-bonding film and to exhibit good adhesiveness. Moreover, the thermal conductivity improvement effect by addition of a heat conductive particle can be made more favorable by the average particle diameter of the said heat conductive particle being 10 micrometers or less. Further, by setting the average particle size of the thermally conductive particles to 10 μm or less, the thickness of the thermosetting die-bonding film can be reduced, and as a result, the semiconductor chip can be highly laminated, and the thermosetting type Generation | occurrence | production of the chip crack by heat conductive particle protruding from a die-bonding film can be prevented.

前記構成においては、熱可塑性樹脂と熱硬化性樹脂とを含有し、
前記熱硬化性樹脂の含有重量部をAとし、前熱可塑性樹脂の含有重量部をBとしたときに、A/Bが5以上であることが好ましい。
In the above-mentioned configuration, it contains a thermoplastic resin and a thermosetting resin,
When the content part by weight of the thermosetting resin is A and the content part by weight of the pre-thermoplastic resin is B, it is preferable that A / B is 5 or more.

熱可塑性樹脂と熱硬化性樹脂とを含有し、前記熱硬化性樹脂の含有重量部をAとし、前熱可塑性樹脂の含有重量部をBとしたときに、A/Bが5以上であると、130℃において、ずり速度50(1/秒)で測定される溶融粘度を低下させ易い。   When the thermoplastic resin and the thermosetting resin are contained, the content part by weight of the thermosetting resin is A, and the content part by weight of the pre-thermoplastic resin is B, A / B is 5 or more. At 130 ° C., the melt viscosity measured at a shear rate of 50 (1 / second) is likely to be lowered.

前記構成において、前記熱硬化性樹脂は、軟化点が100℃以下のものを含むことが好ましい。   The said structure WHEREIN: It is preferable that the said thermosetting resin contains a softening point of 100 degrees C or less.

前記熱硬化性樹脂が、軟化点が100℃以下のものを含むと、熱硬化型ダイボンドフィルム低速せん断応力(例えば、ずり速度5(1/秒))印加下での130℃での溶融粘度、すなわち、圧力を加えない状態での熱硬化型ダイボンドフィルムの130℃での溶融粘度を低下させ易い。その結果、高速せん断応力を加えた際の粘度の低下量が少ない場合であっても、被着体の凹凸に十分に追従でき、ボイドの発生を抑制することができる。   When the thermosetting resin contains a softening point of 100 ° C. or less, a melt viscosity at 130 ° C. under application of a thermosetting die-bonding film low-speed shear stress (for example, shear rate 5 (1 / second)), That is, it is easy to reduce the melt viscosity at 130 ° C. of the thermosetting die-bonding film without applying pressure. As a result, even when the amount of decrease in viscosity when applying high-speed shear stress is small, it is possible to sufficiently follow the unevenness of the adherend and suppress the generation of voids.

前記構成において、前記熱硬化性樹脂は、室温で液状のものを含むことが好ましい。   The said structure WHEREIN: It is preferable that the said thermosetting resin contains a liquid thing at room temperature.

前記熱硬化性樹脂が、室温で液状のものを含むと、被着体の凹凸により十分に追従でき、ボイドの発生を抑制することができる。なお、室温で液状とは、ずり速度5(1/秒)で測定される23℃での粘度が1〜50万mPa・sのものをいう。   If the thermosetting resin contains a liquid at room temperature, it can sufficiently follow the unevenness of the adherend, and the generation of voids can be suppressed. The liquid state at room temperature means one having a viscosity at 23 ° C. of 1 to 500,000 mPa · s measured at a shear rate of 5 (1 / second).

また、本発明に係る半導体装置の製造方法は、前記に記載の熱硬化型ダイボンドフィルムを準備する工程と、
前記熱硬化型ダイボンドフィルムを介して、前記半導体チップを被着体上にダイボンドするダイボンド工程とを含むことを特徴とする。
Moreover, the manufacturing method of the semiconductor device according to the present invention includes a step of preparing the thermosetting die-bonding film described above,
A die-bonding step of die-bonding the semiconductor chip on an adherend through the thermosetting die-bonding film.

前記構成によれば、前記熱硬化型ダイボンドフィルムが、熱伝導率が12W/m・K以上の熱伝導性粒子を、熱硬化型ダイボンドフィルム全体に対して75重量%以上含有しており、熱硬化後の熱伝導率が1W/m・K以上であるため、当該熱硬化型ダイボンドフィルムを用いて製造される半導体装置は、放熱性に優れる。
また、130℃において、ずり速度50(1/秒)で測定される溶融粘度、すなわち、130℃における高速せん断時の溶融粘度が200Pa・s以下であるため、熱硬化型ダイボンドフィルムを被着体に貼り付ける際の圧力により、熱硬化型ダイボンドフィルムの粘度が低下する。従って、プリント配線基板などの被着体の凹凸に十分に追従でき、ボイドの発生を抑制することができる。
According to the said structure, the said thermosetting type die-bonding film contains 75weight% or more of heat conductive particles with a heat conductivity of 12 W / m * K or more with respect to the whole thermosetting type die-bonding film, Since the thermal conductivity after curing is 1 W / m · K or more, the semiconductor device manufactured using the thermosetting die-bonding film is excellent in heat dissipation.
Further, since the melt viscosity measured at a shear rate of 50 (1 / second) at 130 ° C., that is, the melt viscosity at high-speed shear at 130 ° C. is 200 Pa · s or less, the thermosetting die bond film is attached to the adherend. The viscosity of the thermosetting die-bonding film decreases due to the pressure applied to the film. Accordingly, it is possible to sufficiently follow the unevenness of the adherend such as a printed wiring board and to suppress the generation of voids.

また、本発明に係るダイシングシート付きダイボンドフィルムは、前記の課題を解決する為に、前記に記載の熱硬化型ダイボンドフィルムが、基材上に粘着剤層が積層されたダイシングシート上に積層されていることを特徴とする。   Moreover, the die-bonding film with a dicing sheet according to the present invention is formed by laminating the thermosetting die-bonding film described above on a dicing sheet in which an adhesive layer is laminated on a substrate. It is characterized by.

また、本発明に係る半導体装置の製造方法は、前記に記載のダイシングシート付きダイボンドフィルムを準備する工程と、
前記ダイシングシート付きダイボンドフィルムの熱硬化型ダイボンドフィルムと、半導体ウェハの裏面とを貼り合わせる貼り合わせ工程と、
前記半導体ウェハを前記熱硬化型ダイボンドフィルムと共にダイシングして、チップ状の半導体チップを形成するダイシング工程と、
前記半導体チップを、前記ダイシングシート付きダイボンドフィルムから前記熱硬化型ダイボンドフィルムと共にピックアップするピックアップ工程と、
前記熱硬化型ダイボンドフィルムを介して、前記半導体チップを被着体上にダイボンドするダイボンド工程とを含むことを特徴とする。
Moreover, the method of manufacturing a semiconductor device according to the present invention includes a step of preparing the die bond film with a dicing sheet as described above,
A bonding step of bonding the thermosetting die-bonding film of the die-bonding film with the dicing sheet and the back surface of the semiconductor wafer;
Dicing the semiconductor wafer together with the thermosetting die bond film to form a chip-shaped semiconductor chip;
A pick-up step of picking up the semiconductor chip together with the thermosetting die-bonding film from the die-bonding film with the dicing sheet;
A die-bonding step of die-bonding the semiconductor chip on an adherend through the thermosetting die-bonding film.

前記構成によれば、熱伝導率が12W/m・K以上の熱伝導性粒子を、熱硬化型ダイボンドフィルム全体に対して75重量%以上含有しており、熱硬化後の熱伝導率が1W/m・K以上であるため、当該熱硬化型ダイボンドフィルムを用いて製造される半導体装置は、放熱性に優れる。
また、前記熱硬化型ダイボンドフィルムの130℃における高速せん断時の溶融粘度、すなわち、130℃において、ずり速度50(1/秒)で測定される溶融粘度が200Pa・s以下であるため、熱硬化型ダイボンドフィルムを被着体に貼り付ける際の圧力により、熱硬化型ダイボンドフィルムの粘度が低下する。従って、プリント配線基板などの被着体の凹凸に十分に追従でき、ボイドの発生を抑制することができる。
According to the said structure, the heat conductivity of 12 W / m * K or more is contained 75weight% or more with respect to the whole thermosetting die-bonding film, and the heat conductivity after thermosetting is 1W. Since it is / m · K or more, the semiconductor device manufactured using the thermosetting die-bonding film is excellent in heat dissipation.
Moreover, since the melt viscosity at the time of high-speed shearing at 130 ° C. of the thermosetting die-bonding film, that is, the melt viscosity measured at a shear rate of 50 (1 / second) at 130 ° C. is 200 Pa · s or less, thermosetting The viscosity of the thermosetting die-bonding film is lowered by the pressure when the die-bonding film is attached to the adherend. Accordingly, it is possible to sufficiently follow the unevenness of the adherend such as a printed wiring board and to suppress the generation of voids.

本発明の一実施形態に係るダイシングシート付きダイボンドフィルムを示す断面模式図である。It is a cross-sectional schematic diagram which shows the die-bonding film with a dicing sheet which concerns on one Embodiment of this invention. 本発明の他の実施形態に係るダイシングシート付きダイボンドフィルムを示す断面模式図である。It is a cross-sectional schematic diagram which shows the die-bonding film with a dicing sheet which concerns on other embodiment of this invention. 本実施形態に係る半導体装置の一製造方法を説明するための断面模式図である。It is a cross-sectional schematic diagram for demonstrating one manufacturing method of the semiconductor device which concerns on this embodiment.

(ダイシングシート付きダイボンドフィルム)
本発明の一実施形態に係る熱硬化型ダイボンドフィルム(以下、「ダイボンドフィルム」ともいう)、及び、ダイシングシート付きダイボンドフィルムについて、以下に説明する。本実施形態に係るダイボンドフィルムは、以下に説明するダイシングシート付きダイボンドフィルムにおいて、ダイシングシートが貼り合わせられていない状態のものを挙げることができる。従って、以下では、ダイシングシート付きダイボンドフィルムについて説明し、ダイボンドフィルムについては、その中で説明することとする。図1は、本発明の一実施形態に係るダイシングシート付きダイボンドフィルムを示す断面模式図である。図2は、本発明の他の実施形態に係る他のダイシングシート付きダイボンドフィルムを示す断面模式図である。
(Die bond film with dicing sheet)
A thermosetting die bond film (hereinafter also referred to as “die bond film”) and a die bond film with a dicing sheet according to an embodiment of the present invention will be described below. The die bond film which concerns on this embodiment can mention the thing of the state in which the dicing sheet is not bonded together in the die bond film with a dicing sheet demonstrated below. Therefore, hereinafter, a die bond film with a dicing sheet will be described, and the die bond film will be described therein. FIG. 1 is a schematic cross-sectional view showing a die bond film with a dicing sheet according to an embodiment of the present invention. FIG. 2 is a schematic cross-sectional view showing another die-bonding film with a dicing sheet according to another embodiment of the present invention.

図1に示すように、ダイシングシート付きダイボンドフィルム10は、ダイシングシート11上に熱硬化型ダイボンドフィルム3が積層された構成を有する。ダイシングシート11は基材1上に粘着剤層2を積層して構成されており、ダイボンドフィルム3はその粘着剤層2上に設けられている。また本発明は、図2に示すダイシングシート付きダイボンドフィルム12のように、ワーク貼り付け部分にのみダイボンドフィルム3’を形成した構成であってもよい。   As shown in FIG. 1, a die bond film 10 with a dicing sheet has a configuration in which a thermosetting die bond film 3 is laminated on a dicing sheet 11. The dicing sheet 11 is configured by laminating the pressure-sensitive adhesive layer 2 on the base material 1, and the die bond film 3 is provided on the pressure-sensitive adhesive layer 2. Moreover, the structure which formed the die-bonding film 3 'only in the workpiece | work affixing part may be sufficient as this invention like the die-bonding film 12 with a dicing sheet shown in FIG.

前記基材1は紫外線透過性を有し、かつダイシングシート付きダイボンドフィルム10、12の強度母体となるものである。例えば、低密度ポリエチレン、直鎖状ポリエチレン、中密度ポリエチレン、高密度ポリエチレン、超低密度ポリエチレン、ランダム共重合ポリプロピレン、ブロック共重合ポリプロピレン、ホモポリプロレン、ポリブテン、ポリメチルペンテン等のポリオレフィン、エチレン−酢酸ビニル共重合体、アイオノマー樹脂、エチレン−(メタ)アクリル酸共重合体、エチレン−(メタ)アクリル酸エステル(ランダム、交互)共重合体、エチレン−ブテン共重合体、エチレン−ヘキセン共重合体、ポリウレタン、ポリエチレンテレフタレート、ポリエチレンナフタレート等のポリエステル、ポリカーボネート、ポリイミド、ポリエーテルエーテルケトン、ポリイミド、ポリエーテルイミド、ポリアミド、全芳香族ポリアミド、ポリフェニルスルフイド、アラミド(紙)、ガラス、ガラスクロス、フッ素樹脂、ポリ塩化ビニル、ポリ塩化ビニリデン、セルロース系樹脂、シリコーン樹脂、金属(箔)、紙等が挙げられる。   The base material 1 has ultraviolet transparency and serves as a strength matrix for the die bond films 10 and 12 with a dicing sheet. For example, polyolefins such as low density polyethylene, linear polyethylene, medium density polyethylene, high density polyethylene, ultra low density polyethylene, random copolymer polypropylene, block copolymer polypropylene, homopolyprolene, polybutene, polymethylpentene, ethylene-acetic acid Vinyl copolymer, ionomer resin, ethylene- (meth) acrylic acid copolymer, ethylene- (meth) acrylic acid ester (random, alternating) copolymer, ethylene-butene copolymer, ethylene-hexene copolymer, Polyester such as polyurethane, polyethylene terephthalate, polyethylene naphthalate, polycarbonate, polyimide, polyetheretherketone, polyimide, polyetherimide, polyamide, wholly aromatic polyamide, polyphenylsulfur De, aramid (paper), glass, glass cloth, fluorine resin, polyvinyl chloride, polyvinylidene chloride, cellulose resin, silicone resin, metal (foil), paper, and the like.

また基材1の材料としては、前記樹脂の架橋体等のポリマーが挙げられる。前記プラスチックフィルムは、無延伸で用いてもよく、必要に応じて一軸又は二軸の延伸処理を施したものを用いてもよい。延伸処理等により熱収縮性を付与した樹脂シートによれば、ダイシング後にその基材1を熱収縮させることにより粘着剤層2とダイボンドフィルム3、3’との接着面積を低下させて、半導体チップの回収の容易化を図ることができる。   Moreover, as a material of the base material 1, polymers, such as the crosslinked body of the said resin, are mentioned. The plastic film may be used unstretched or may be uniaxially or biaxially stretched as necessary. According to the resin sheet to which heat shrinkability is imparted by stretching treatment or the like, the adhesive area between the pressure-sensitive adhesive layer 2 and the die bond films 3 and 3 ′ is reduced by thermally shrinking the base material 1 after dicing, so that the semiconductor chip Can be easily recovered.

基材1の表面は、隣接する層との密着性、保持性等を高めるため、慣用の表面処理、例えば、クロム酸処理、オゾン暴露、火炎暴露、高圧電撃暴露、イオン化放射線処理等の化学的又は物理的処理、下塗剤(例えば、後述する粘着物質)によるコーティング処理を施すことができる。前記基材1は、同種又は異種のものを適宜に選択して使用することができ、必要に応じて数種をブレンドしたものを用いることができる。   The surface of the substrate 1 is chemically treated by conventional surface treatments such as chromic acid treatment, ozone exposure, flame exposure, high piezoelectric impact exposure, ionizing radiation treatment, etc. in order to improve adhesion and retention with adjacent layers. Alternatively, a physical treatment or a coating treatment with a primer (for example, an adhesive substance described later) can be performed. The base material 1 can be used by appropriately selecting the same kind or different kinds, and a blend of several kinds can be used as necessary.

基材1の厚さは、特に制限されず適宜に決定できるが、一般的には5〜200μm程度である。   The thickness of the substrate 1 is not particularly limited and can be appropriately determined, but is generally about 5 to 200 μm.

粘着剤層2の形成に用いる粘着剤としては特に制限されず、例えば、アクリル系粘着剤、ゴム系粘着剤等の一般的な感圧性粘着剤を用いることができる。前記感圧性粘着剤としては、半導体ウェハやガラス等の汚染をきらう電子部品の超純水やアルコール等の有機溶剤による清浄洗浄性等の点から、アクリル系ポリマーをベースポリマーとするアクリル系粘着剤が好ましい。   It does not restrict | limit especially as an adhesive used for formation of the adhesive layer 2, For example, common pressure sensitive adhesives, such as an acrylic adhesive and a rubber adhesive, can be used. The pressure-sensitive adhesive is an acrylic pressure-sensitive adhesive based on an acrylic polymer from the standpoint of cleanability with an organic solvent such as ultrapure water or alcohol for electronic components that are difficult to contaminate semiconductor wafers and glass. Is preferred.

前記アクリル系ポリマーとしては、例えば、(メタ)アクリル酸アルキルエステル(例えば、メチルエステル、エチルエステル、プロピルエステル、イソプロピルエステル、ブチルエステル、イソブチルエステル、s−ブチルエステル、t−ブチルエステル、ペンチルエステル、イソペンチルエステル、ヘキシルエステル、ヘプチルエステル、オクチルエステル、2−エチルヘキシルエステル、イソオクチルエステル、ノニルエステル、デシルエステル、イソデシルエステル、ウンデシルエステル、ドデシルエステル、トリデシルエステル、テトラデシルエステル、ヘキサデシルエステル、オクタデシルエステル、エイコシルエステル等のアルキル基の炭素数1〜30、特に炭素数4〜18の直鎖状又は分岐鎖状のアルキルエステル等)及び(メタ)アクリル酸シクロアルキルエステル(例えば、シクロペンチルエステル、シクロヘキシルエステル等)の1種又は2種以上を単量体成分として用いたアクリル系ポリマー等が挙げられる。なお、(メタ)アクリル酸エステルとはアクリル酸エステル及び/又はメタクリル酸エステルをいい、本発明の(メタ)とは全て同様の意味である。   Examples of the acrylic polymer include (meth) acrylic acid alkyl esters (for example, methyl ester, ethyl ester, propyl ester, isopropyl ester, butyl ester, isobutyl ester, s-butyl ester, t-butyl ester, pentyl ester, Isopentyl ester, hexyl ester, heptyl ester, octyl ester, 2-ethylhexyl ester, isooctyl ester, nonyl ester, decyl ester, isodecyl ester, undecyl ester, dodecyl ester, tridecyl ester, tetradecyl ester, hexadecyl ester , Octadecyl esters, eicosyl esters, etc., alkyl groups having 1 to 30 carbon atoms, especially 4 to 18 carbon linear or branched alkyl esters, etc.) and Meth) acrylic acid cycloalkyl esters (e.g., cyclopentyl ester, acrylic polymers such as one or more was used as a monomer component of the cyclohexyl ester etc.). In addition, (meth) acrylic acid ester means acrylic acid ester and / or methacrylic acid ester, and (meth) of the present invention has the same meaning.

前記アクリル系ポリマーは、凝集力、耐熱性等の改質を目的として、必要に応じ、前記(メタ)アクリル酸アルキルエステル又はシクロアルキルエステルと共重合可能な他のモノマー成分に対応する単位を含んでいてもよい。この様なモノマー成分として、例えば、アクリル酸、メタクリル酸、カルボキシエチル(メタ)アクリレート、カルボキシペンチル(メタ)アクリレート、イタコン酸、マレイン酸、フマル酸、クロトン酸等のカルボキシル基含有モノマー;無水マレイン酸、無水イタコン酸等の酸無水物モノマー;(メタ)アクリル酸2−ヒドロキシエチル、(メタ)アクリル酸2−ヒドロキシプロピル、(メタ)アクリル酸4−ヒドロキシブチル、(メタ)アクリル酸6−ヒドロキシヘキシル、(メタ)アクリル酸8−ヒドロキシオクチル、(メタ)アクリル酸10−ヒドロキシデシル、(メタ)アクリル酸12−ヒドロキシラウリル、(4−ヒドロキシメチルシクロヘキシル)メチル(メタ)アクリレート等のヒドロキシル基含有モノマー;スチレンスルホン酸、アリルスルホン酸、2−(メタ)アクリルアミド−2−メチルプロパンスルホン酸、(メタ)アクリルアミドプロパンスルホン酸、スルホプロピル(メタ)アクリレート、(メタ)アクリロイルオキシナフタレンスルホン酸等のスルホン酸基含有モノマー;2−ヒドロキシエチルアクリロイルホスフェート等のリン酸基含有モノマー;アクリルアミド、アクリロニトリル等が挙げられる。これら共重合可能なモノマー成分は、1種又は2種以上使用できる。これら共重合可能なモノマーの使用量は、全モノマー成分の40重量%以下が好ましい。   The acrylic polymer contains units corresponding to other monomer components copolymerizable with the (meth) acrylic acid alkyl ester or cycloalkyl ester, if necessary, for the purpose of modifying cohesive force, heat resistance and the like. You may go out. Examples of such monomer components include, for example, carboxyl group-containing monomers such as acrylic acid, methacrylic acid, carboxyethyl (meth) acrylate, carboxypentyl (meth) acrylate, itaconic acid, maleic acid, fumaric acid, and crotonic acid; maleic anhydride Acid anhydride monomers such as itaconic anhydride; 2-hydroxyethyl (meth) acrylate, 2-hydroxypropyl (meth) acrylate, 4-hydroxybutyl (meth) acrylate, 6-hydroxyhexyl (meth) acrylate Hydroxyl group-containing monomers such as 8-hydroxyoctyl (meth) acrylate, 10-hydroxydecyl (meth) acrylate, 12-hydroxylauryl (meth) acrylate, (4-hydroxymethylcyclohexyl) methyl (meth) acrylate; Styrene Contains sulfonic acid groups such as phonic acid, allylsulfonic acid, 2- (meth) acrylamide-2-methylpropanesulfonic acid, (meth) acrylamidepropanesulfonic acid, sulfopropyl (meth) acrylate, (meth) acryloyloxynaphthalenesulfonic acid Monomers; Phosphoric acid group-containing monomers such as 2-hydroxyethyl acryloyl phosphate; acrylamide, acrylonitrile and the like. One or more of these copolymerizable monomer components can be used. The amount of these copolymerizable monomers used is preferably 40% by weight or less based on the total monomer components.

さらに、前記アクリル系ポリマーは、架橋させるため、多官能性モノマー等も、必要に応じて共重合用モノマー成分として含むことができる。この様な多官能性モノマーとして、例えば、ヘキサンジオールジ(メタ)アクリレート、(ポリ)エチレングリコールジ(メタ)アクリレート、(ポリ)プロピレングリコールジ(メタ)アクリレート、ネオペンチルグリコールジ(メタ)アクリレート、ペンタエリスリトールジ(メタ)アクリレート、トリメチロールプロパントリ(メタ)アクリレート、ペンタエリスリトールトリ(メタ)アクリレート、ジペンタエリスリトールヘキサ(メタ)アクリレート、エポキシ(メタ)アクリレート、ポリエステル(メタ)アクリレート、ウレタン(メタ)アクリレート等が挙げられる。これらの多官能性モノマーも1種又は2種以上用いることができる。多官能性モノマーの使用量は、粘着特性等の点から、全モノマー成分の30重量%以下が好ましい。   Furthermore, since the acrylic polymer is crosslinked, a polyfunctional monomer or the like can be included as a monomer component for copolymerization as necessary. Examples of such polyfunctional monomers include hexanediol di (meth) acrylate, (poly) ethylene glycol di (meth) acrylate, (poly) propylene glycol di (meth) acrylate, neopentyl glycol di (meth) acrylate, Pentaerythritol di (meth) acrylate, trimethylolpropane tri (meth) acrylate, pentaerythritol tri (meth) acrylate, dipentaerythritol hexa (meth) acrylate, epoxy (meth) acrylate, polyester (meth) acrylate, urethane (meth) An acrylate etc. are mentioned. These polyfunctional monomers can also be used alone or in combination of two or more. The amount of the polyfunctional monomer used is preferably 30% by weight or less of the total monomer components from the viewpoint of adhesive properties and the like.

前記アクリル系ポリマーは、単一モノマー又は2種以上のモノマー混合物を重合に付すことにより得られる。重合は、溶液重合、乳化重合、塊状重合、懸濁重合等の何れの方式で行うこともできる。清浄な被着体への汚染防止等の点から、低分子量物質の含有量が小さいのが好ましい。この点から、アクリル系ポリマーの数平均分子量は、好ましくは10万以上、さらに好ましくは20万〜300万程度であり、特に好ましくは30万〜100万程度である。   The acrylic polymer can be obtained by subjecting a single monomer or a mixture of two or more monomers to polymerization. The polymerization can be performed by any method such as solution polymerization, emulsion polymerization, bulk polymerization, suspension polymerization and the like. From the viewpoint of preventing contamination of a clean adherend, the content of the low molecular weight substance is preferably small. From this point, the number average molecular weight of the acrylic polymer is preferably 100,000 or more, more preferably about 200,000 to 3,000,000, and particularly preferably about 300,000 to 1,000,000.

また、前記粘着剤には、ベースポリマーであるアクリル系ポリマー等の数平均分子量を高めるため、外部架橋剤を適宜に採用することもできる。外部架橋方法の具体的手段としては、ポリイソシアネート化合物、エポキシ化合物、アジリジン化合物、メラミン系架橋剤等のいわゆる架橋剤を添加し反応させる方法が挙げられる。外部架橋剤を使用する場合、その使用量は、架橋すべきベースポリマーとのバランスにより、さらには、粘着剤としての使用用途によって適宜決定される。一般的には、前記ベースポリマー100重量部に対して、5重量部程度以下、さらには0.1〜5重量部配合するのが好ましい。さらに、粘着剤には、必要により、前記成分のほかに、従来公知の各種の粘着付与剤、老化防止剤等の添加剤を用いてもよい。   In addition, an external cross-linking agent can be appropriately employed for the pressure-sensitive adhesive in order to increase the number average molecular weight of an acrylic polymer as a base polymer. Specific examples of the external crosslinking method include a method of adding a so-called crosslinking agent such as a polyisocyanate compound, an epoxy compound, an aziridine compound, a melamine crosslinking agent, and reacting them. When using an external cross-linking agent, the amount used is appropriately determined depending on the balance with the base polymer to be cross-linked, and further depending on the intended use as an adhesive. In general, about 5 parts by weight or less, further 0.1 to 5 parts by weight is preferably blended with respect to 100 parts by weight of the base polymer. Furthermore, you may use additives, such as conventionally well-known various tackifiers and anti-aging agent, other than the said component as needed to an adhesive.

粘着剤層2は放射線硬化型粘着剤により形成することができる。放射線硬化型粘着剤は、紫外線等の放射線の照射により架橋度を増大させてその粘着力を容易に低下させることができ、図2に示す粘着剤層2のワーク貼り付け部分に対応する部分2aのみを放射線照射することにより他の部分2bとの粘着力の差を設けることができる。   The pressure-sensitive adhesive layer 2 can be formed of a radiation curable pressure-sensitive adhesive. The radiation curable pressure-sensitive adhesive can increase the degree of cross-linking by irradiation with radiation such as ultraviolet rays, and can easily reduce its adhesive strength, and a portion 2a corresponding to the work pasting portion of the pressure-sensitive adhesive layer 2 shown in FIG. The difference in adhesive strength with the other part 2b can be provided by irradiating only with radiation.

また、図2に示すダイボンドフィルム3’に合わせて放射線硬化型の粘着剤層2を硬化させることにより、粘着力が著しく低下した前記部分2aを容易に形成できる。硬化し、粘着力の低下した前記部分2aにダイボンドフィルム3’が貼付けられるため、粘着剤層2の前記部分2aとダイボンドフィルム3’との界面は、ピックアップ時に容易に剥がれる性質を有する。一方、放射線を照射していない部分は十分な粘着力を有しており、前記部分2bを形成する。なお、粘着剤層への放射線の照射は、ダイシング後であってかつピックアップ前に行ってもよい。   Further, by curing the radiation curable pressure-sensitive adhesive layer 2 in accordance with the die bond film 3 ′ shown in FIG. 2, the portion 2 a having a significantly reduced adhesive force can be easily formed. Since the die bond film 3 ′ is attached to the portion 2 a that has been cured and has reduced adhesive strength, the interface between the portion 2 a and the die bond film 3 ′ of the pressure-sensitive adhesive layer 2 has a property of being easily peeled off during pick-up. On the other hand, the portion not irradiated with radiation has a sufficient adhesive force, and forms the portion 2b. In addition, you may perform irradiation of the radiation to an adhesive layer after dicing and before pick-up.

前述の通り、図1に示すダイシングシート付きダイボンドフィルム10の粘着剤層2において、未硬化の放射線硬化型粘着剤により形成されている前記部分2bはダイボンドフィルム3と粘着し、ダイシングする際の保持力を確保できる。この様に放射線硬化型粘着剤は、チップ状ワーク(半導体チップ等)を基板等の被着体に固着するためのダイボンドフィルム3を、接着・剥離のバランスよく支持することができる。図2に示すダイシングシート付きダイボンドフィルム11の粘着剤層2においては、前記部分2bがウェハリングを固定することができる。   As described above, in the pressure-sensitive adhesive layer 2 of the die-bonding film with a dicing sheet 10 shown in FIG. 1, the portion 2 b formed of the uncured radiation-curable pressure-sensitive adhesive adheres to the die-bonding film 3 and is retained when dicing. Power can be secured. In this way, the radiation curable pressure-sensitive adhesive can support the die bond film 3 for fixing a chip-like work (semiconductor chip or the like) to an adherend such as a substrate with a good balance of adhesion and peeling. In the pressure-sensitive adhesive layer 2 of the die-bonding film with a dicing sheet 11 shown in FIG. 2, the portion 2b can fix the wafer ring.

放射線硬化型粘着剤は、炭素−炭素二重結合等の放射線硬化性の官能基を有し、かつ粘着性を示すものを特に制限なく使用することができる。放射線硬化型粘着剤としては、例えば、前記アクリル系粘着剤、ゴム系粘着剤等の一般的な感圧性粘着剤に、放射線硬化性のモノマー成分やオリゴマー成分を配合した添加型の放射線硬化型粘着剤を例示できる。   As the radiation-curable pressure-sensitive adhesive, those having a radiation-curable functional group such as a carbon-carbon double bond and exhibiting adhesiveness can be used without particular limitation. As the radiation curable pressure sensitive adhesive, for example, an addition type radiation curable pressure sensitive adhesive in which a radiation curable monomer component or an oligomer component is blended with a general pressure sensitive pressure sensitive adhesive such as an acrylic pressure sensitive adhesive or a rubber pressure sensitive adhesive. An agent can be illustrated.

配合する放射線硬化性のモノマー成分としては、例えば、ウレタンオリゴマー、ウレタン(メタ)アクリレート、トリメチロールプロパントリ(メタ)アクリレート、テトラメチロールメタンテトラ(メタ)アクリレート、ペンタエリスリトールトリ(メタ)アクリレート、ペンタエリストールテトラ(メタ)アクリレート、ジペンタエリストールモノヒドロキシペンタ(メタ)アクリレート、ジペンタエリスリトールヘキサ(メタ)アクリレート、1,4−ブタンジオールジ(メタ)アクリレート等が挙げられる。また放射線硬化性のオリゴマー成分はウレタン系、ポリエーテル系、ポリエステル系、ポリカーボネート系、ポリブタジエン系等種々のオリゴマーがあげられ、その分子量が100〜30000程度の範囲のものが適当である。放射線硬化性のモノマー成分やオリゴマー成分の配合量は、前記粘着剤層の種類に応じて、粘着剤層の粘着力を低下できる量を、適宜に決定することができる。一般的には、粘着剤を構成するアクリル系ポリマー等のベースポリマー100重量部に対して、例えば5〜500重量部、好ましくは40〜150重量部程度である。   Examples of the radiation curable monomer component to be blended include urethane oligomer, urethane (meth) acrylate, trimethylolpropane tri (meth) acrylate, tetramethylolmethane tetra (meth) acrylate, pentaerythritol tri (meth) acrylate, and pentaerythritol. Examples include stall tetra (meth) acrylate, dipentaerystol monohydroxypenta (meth) acrylate, dipentaerythritol hexa (meth) acrylate, 1,4-butanediol di (meth) acrylate, and the like. Examples of the radiation curable oligomer component include various oligomers such as urethane, polyether, polyester, polycarbonate, and polybutadiene, and those having a molecular weight in the range of about 100 to 30,000 are suitable. The compounding amount of the radiation-curable monomer component or oligomer component can be appropriately determined in accordance with the type of the pressure-sensitive adhesive layer, and the amount capable of reducing the adhesive strength of the pressure-sensitive adhesive layer. Generally, the amount is, for example, about 5 to 500 parts by weight, preferably about 40 to 150 parts by weight with respect to 100 parts by weight of the base polymer such as an acrylic polymer constituting the pressure-sensitive adhesive.

また、放射線硬化型粘着剤としては、前記説明した添加型の放射線硬化型粘着剤のほかに、ベースポリマーとして、炭素−炭素二重結合をポリマー側鎖又は主鎖中もしくは主鎖末端に有するものを用いた内在型の放射線硬化型粘着剤が挙げられる。内在型の放射線硬化型粘着剤は、低分子成分であるオリゴマー成分等を含有する必要がなく、又は多くは含まないため、経時的にオリゴマー成分等が粘着剤在中を移動することなく、安定した層構造の粘着剤層を形成することができるため好ましい。   In addition to the additive-type radiation curable adhesive described above, the radiation curable pressure-sensitive adhesive has a carbon-carbon double bond in the polymer side chain or main chain or at the main chain terminal as a base polymer. Intrinsic radiation curable pressure sensitive adhesives using Intrinsic radiation curable adhesives do not need to contain oligomer components, which are low molecular components, or do not contain many, so the oligomer components do not move through the adhesive over time and are stable. This is preferable because an adhesive layer having a layered structure can be formed.

前記炭素−炭素二重結合を有するベースポリマーは、炭素−炭素二重結合を有し、かつ粘着性を有するものを特に制限なく使用できる。この様なベースポリマーとしては、アクリル系ポリマーを基本骨格とするものが好ましい。アクリル系ポリマーの基本骨格としては、前記例示したアクリル系ポリマーが挙げられる。   As the base polymer having a carbon-carbon double bond, those having a carbon-carbon double bond and having adhesiveness can be used without particular limitation. As such a base polymer, those having an acrylic polymer as a basic skeleton are preferable. Examples of the basic skeleton of the acrylic polymer include the acrylic polymers exemplified above.

前記アクリル系ポリマーへの炭素−炭素二重結合の導入法は特に制限されず、様々な方法を採用できるが、炭素−炭素二重結合はポリマー側鎖に導入するのが分子設計の点で容易である。例えば、予め、アクリル系ポリマーに官能基を有するモノマーを共重合した後、この官能基と反応しうる官能基及び炭素−炭素二重結合を有する化合物を、炭素−炭素二重結合の放射線硬化性を維持したまま縮合又は付加反応させる方法が挙げられる。   The method for introducing the carbon-carbon double bond into the acrylic polymer is not particularly limited, and various methods can be adopted, but it is easy in terms of molecular design to introduce the carbon-carbon double bond into the polymer side chain. It is. For example, after a monomer having a functional group is previously copolymerized with an acrylic polymer, a compound having a functional group capable of reacting with the functional group and a carbon-carbon double bond is converted into a radiation curable carbon-carbon double bond. A method of performing condensation or addition reaction while maintaining the above.

これら官能基の組合せの例としては、カルボン酸基とエポキシ基、カルボン酸基とアジリジル基、ヒドロキシル基とイソシアネート基等が挙げられる。これら官能基の組合せのなかでも反応追跡の容易さから、ヒドロキシル基とイソシアネート基との組合せが好適である。また、これら官能基の組み合わせにより、前記炭素−炭素二重結合を有するアクリル系ポリマーを生成するような組合せであれば、官能基はアクリル系ポリマーと前記化合物のいずれの側にあってもよいが、前記の好ましい組み合わせでは、アクリル系ポリマーがヒドロキシル基を有し、前記化合物がイソシアネート基を有する場合が好適である。この場合、炭素−炭素二重結合を有するイソシアネート化合物としては、例えば、メタクリロイルイソシアネート、2−メタクリロイルオキシエチルイソシアネート、m−イソプロペニル−α,α−ジメチルベンジルイソシアネート等が挙げられる。また、アクリル系ポリマーとしては、前記例示のヒドロキシ基含有モノマーや2−ヒドロキシエチルビニルエーテル、4−ヒドロキシブチルビニルエーテル、ジエチレングルコールモノビニルエーテルのエーテル系化合物等を共重合したものが用いられる。   Examples of combinations of these functional groups include carboxylic acid groups and epoxy groups, carboxylic acid groups and aziridyl groups, hydroxyl groups and isocyanate groups, and the like. Among these combinations of functional groups, a combination of a hydroxyl group and an isocyanate group is preferable because of easy tracking of the reaction. Moreover, the functional group may be on either side of the acrylic polymer and the compound as long as the acrylic polymer having the carbon-carbon double bond is generated by a combination of these functional groups. In the preferable combination, it is preferable that the acrylic polymer has a hydroxyl group and the compound has an isocyanate group. In this case, examples of the isocyanate compound having a carbon-carbon double bond include methacryloyl isocyanate, 2-methacryloyloxyethyl isocyanate, m-isopropenyl-α, α-dimethylbenzyl isocyanate, and the like. Further, as the acrylic polymer, those obtained by copolymerizing the above-exemplified hydroxy group-containing monomers, ether compounds of 2-hydroxyethyl vinyl ether, 4-hydroxybutyl vinyl ether, diethylene glycol monovinyl ether, or the like are used.

前記内在型の放射線硬化型粘着剤は、前記炭素−炭素二重結合を有するベースポリマー(特にアクリル系ポリマー)を単独で使用することができるが、特性を悪化させない程度に前記放射線硬化性のモノマー成分やオリゴマー成分を配合することもできる。放射線硬化性のオリゴマー成分等は、通常ベースポリマー100重量部に対して30重量部の範囲内であり、好ましくは0〜10重量部の範囲である。   As the intrinsic radiation curable pressure-sensitive adhesive, the base polymer (particularly acrylic polymer) having the carbon-carbon double bond can be used alone, but the radiation curable monomer does not deteriorate the characteristics. Components and oligomer components can also be blended. The radiation-curable oligomer component or the like is usually in the range of 30 parts by weight, preferably in the range of 0 to 10 parts by weight with respect to 100 parts by weight of the base polymer.

前記放射線硬化型粘着剤には、紫外線等により硬化させる場合には光重合開始剤を含有させる。光重合開始剤としては、例えば、4−(2−ヒドロキシエトキシ)フェニル(2−ヒドロキシ−2−プロピル)ケトン、α−ヒドロキシ−α,α’−ジメチルアセトフェノン、2−メチル−2−ヒドロキシプロピオフェノン、1−ヒドロキシシクロヘキシルフェニルケトン等のα−ケトール系化合物;メトキシアセトフェノン、2,2−ジメトキシ−2−フェニルアセトフエノン、2,2−ジエトキシアセトフェノン、2−メチル−1−[4−(メチルチオ)−フェニル]−2−モルホリノプロパン−1等のアセトフェノン系化合物;ベンゾインエチルエーテル、ベンゾインイソプロピルエーテル、アニソインメチルエーテル等のベンゾインエーテル系化合物;ベンジルジメチルケタール等のケタール系化合物;2−ナフタレンスルホニルクロリド等の芳香族スルホニルクロリド系化合物;1−フェノン−1,1―プロパンジオン−2−(o−エトキシカルボニル)オキシム等の光活性オキシム系化合物;ベンゾフェノン、ベンゾイル安息香酸、3,3’−ジメチル−4−メトキシベンゾフェノン等のベンゾフェノン系化合物;チオキサンソン、2−クロロチオキサンソン、2−メチルチオキサンソン、2,4−ジメチルチオキサンソン、イソプロピルチオキサンソン、2,4−ジクロロチオキサンソン、2,4−ジエチルチオキサンソン、2,4−ジイソプロピルチオキサンソン等のチオキサンソン系化合物;カンファーキノン;ハロゲン化ケトン;アシルホスフィノキシド;アシルホスフォナート等が挙げられる。光重合開始剤の配合量は、粘着剤を構成するアクリル系ポリマー等のベースポリマー100重量部に対して、例えば0.05〜20重量部程度である。   The radiation curable pressure-sensitive adhesive contains a photopolymerization initiator when cured by ultraviolet rays or the like. Examples of the photopolymerization initiator include 4- (2-hydroxyethoxy) phenyl (2-hydroxy-2-propyl) ketone, α-hydroxy-α, α′-dimethylacetophenone, 2-methyl-2-hydroxypropio Α-ketol compounds such as phenone and 1-hydroxycyclohexyl phenyl ketone; methoxyacetophenone, 2,2-dimethoxy-2-phenylacetophenone, 2,2-diethoxyacetophenone, 2-methyl-1- [4- ( Acetophenone compounds such as methylthio) -phenyl] -2-morpholinopropane-1; benzoin ether compounds such as benzoin ethyl ether, benzoin isopropyl ether and anisoin methyl ether; ketal compounds such as benzyldimethyl ketal; 2-naphthalenesulfonyl Black Aromatic sulfonyl chloride compounds such as 1; photoactive oxime compounds such as 1-phenone-1,1-propanedione-2- (o-ethoxycarbonyl) oxime; benzophenone, benzoylbenzoic acid, 3,3′-dimethyl Benzophenone compounds such as -4-methoxybenzophenone; thioxanthone, 2-chlorothioxanthone, 2-methylthioxanthone, 2,4-dimethylthioxanthone, isopropylthioxanthone, 2,4-dichlorothioxanthone, 2 Thioxanthone compounds such as 1,4-diethylthioxanthone and 2,4-diisopropylthioxanthone; camphorquinone; halogenated ketone; acyl phosphinoxide; acyl phosphonate. The compounding quantity of a photoinitiator is about 0.05-20 weight part with respect to 100 weight part of base polymers, such as an acryl-type polymer which comprises an adhesive.

また放射線硬化型粘着剤としては、例えば、特開昭60−196956号公報に開示されている、不飽和結合を2個以上有する付加重合性化合物、エポキシ基を有するアルコキシシラン等の光重合性化合物と、カルボニル化合物、有機硫黄化合物、過酸化物、アミン、オニウム塩系化合物等の光重合開始剤とを含有するゴム系粘着剤やアクリル系粘着剤等が挙げられる。   Examples of radiation curable pressure-sensitive adhesives include photopolymerizable compounds such as addition polymerizable compounds having two or more unsaturated bonds and alkoxysilanes having an epoxy group disclosed in JP-A-60-196956. And a rubber-based pressure-sensitive adhesive and an acrylic pressure-sensitive adhesive containing a photopolymerization initiator such as a carbonyl compound, an organic sulfur compound, a peroxide, an amine, and an onium salt-based compound.

前記放射線硬化型の粘着剤層2中には、必要に応じて、放射線照射により着色する化合物を含有させることもできる。放射線照射により、着色する化合物を粘着剤層2に含ませることによって、放射線照射された部分のみを着色することができる。すなわち、図1に示すワーク貼り付け部分3aに対応する部分2aを着色することができる。従って、粘着剤層2に放射線が照射されたか否かが目視により直ちに判明することができ、ワーク貼り付け部分3aを認識し易く、ワークの貼り合せが容易である。また光センサー等によって半導体チップを検出する際に、その検出精度が高まり、半導体チップのピックアップ時に誤動作が生ずることがない。   The radiation curable pressure-sensitive adhesive layer 2 can contain a compound that is colored by irradiation with radiation, if necessary. By including a compound to be colored in the pressure-sensitive adhesive layer 2 by irradiation with radiation, only the irradiated portion can be colored. That is, the portion 2a corresponding to the workpiece pasting portion 3a shown in FIG. 1 can be colored. Accordingly, whether or not the pressure-sensitive adhesive layer 2 has been irradiated with radiation can be immediately determined by visual observation, the workpiece pasting portion 3a can be easily recognized, and workpieces can be easily pasted together. In addition, when detecting a semiconductor chip by an optical sensor or the like, the detection accuracy is increased, and no malfunction occurs when the semiconductor chip is picked up.

放射線照射により着色する化合物は、放射線照射前には無色又は淡色であるが、放射線照射により有色となる化合物である。かかる化合物の好ましい具体例としてはロイコ染料が挙げられる。ロイコ染料としては、慣用のトリフェニルメタン系、フルオラン系、フェノチアジン系、オーラミン系、スピロピラン系のものが好ましく用いられる。具体的には3−[N−(p−トリルアミノ)]−7−アニリノフルオラン、3−[N−(p−トリル)−N−メチルアミノ]−7−アニリノフルオラン、3−[N−(p−トリル)−N−エチルアミノ]−7−アニリノフルオラン、3−ジエチルアミノ−6−メチル−7−アニリノフルオラン、クリスタルバイオレットラクトン、4,4’,4”−トリスジメチルアミノトリフエニルメタノール、4,4’,4”−トリスジメチルアミノトリフェニルメタン等が挙げられる。   A compound that is colored by radiation irradiation is a compound that is colorless or light-colored before radiation irradiation, but becomes colored by radiation irradiation. Preferable specific examples of such compounds include leuco dyes. As the leuco dye, conventional triphenylmethane, fluoran, phenothiazine, auramine, and spiropyran dyes are preferably used. Specifically, 3- [N- (p-tolylamino)]-7-anilinofluorane, 3- [N- (p-tolyl) -N-methylamino] -7-anilinofluorane, 3- [ N- (p-tolyl) -N-ethylamino] -7-anilinofluorane, 3-diethylamino-6-methyl-7-anilinofluorane, crystal violet lactone, 4,4 ', 4 "-trisdimethyl Examples include aminotriphenylmethanol, 4,4 ′, 4 ″ -trisdimethylaminotriphenylmethane, and the like.

これらロイコ染料とともに好ましく用いられる顕色剤としては、従来から用いられているフェノールホルマリン樹脂の初期重合体、芳香族カルボン酸誘導体、活性白土等の電子受容体があげられ、さらに、色調を変化させる場合は種々公知の発色剤を組合せて用いることもできる。   Developers preferably used together with these leuco dyes include conventionally used initial polymers of phenol formalin resins, aromatic carboxylic acid derivatives, electron acceptors such as activated clay, and further change the color tone. In some cases, various known color formers can be used in combination.

この様な放射線照射によって着色する化合物は、一旦有機溶媒等に溶解された後に放射線硬化型接着剤中に含ませてもよく、また微粉末状にして当該粘着剤中に含ませてもよい。この化合物の使用割合は、粘着剤層2中に10重量%以下、好ましくは0.01〜10重量%、さらに好ましくは0.5〜5重量%であるのが望ましい。該化合物の割合が10重量%を超えると、粘着剤層2に照射される放射線がこの化合物に吸収されすぎてしまうため、粘着剤層2の前記部分2aの硬化が不十分となり、十分に粘着力が低下しないことがある。一方、充分に着色させるには、該化合物の割合を0.01重量%以上とするのが好ましい。   Such a compound that is colored by irradiation with radiation may be once dissolved in an organic solvent or the like and then included in the radiation-curable adhesive, or may be finely powdered and included in the pressure-sensitive adhesive. The use ratio of this compound is 10% by weight or less in the pressure-sensitive adhesive layer 2, preferably 0.01 to 10% by weight, and more preferably 0.5 to 5% by weight. If the proportion of the compound exceeds 10% by weight, the radiation applied to the pressure-sensitive adhesive layer 2 will be absorbed too much by this compound, so that the portion 2a of the pressure-sensitive adhesive layer 2 will be insufficiently cured and will be sufficiently sticky. Power may not decrease. On the other hand, in order to sufficiently color, it is preferable that the ratio of the compound is 0.01% by weight or more.

粘着剤層2を放射線硬化型粘着剤により形成する場合には、粘着剤層2における前記部分2aの粘着力<その他の部分2bの粘着力、となるように粘着剤層2の一部を放射線照射してもよい。   When the pressure-sensitive adhesive layer 2 is formed of a radiation curable pressure-sensitive adhesive, a part of the pressure-sensitive adhesive layer 2 is radiated so that the pressure-sensitive adhesive strength of the portion 2a in the pressure-sensitive adhesive layer 2 is smaller than the pressure-sensitive adhesive strength of the other portion 2b. It may be irradiated.

前記粘着剤層2に前記部分2aを形成する方法としては、支持基材1に放射線硬化型の粘着剤層2を形成した後、前記部分2aに部分的に放射線を照射し硬化させる方法が挙げられる。部分的な放射線照射は、ワーク貼り付け部分3a以外の部分3b等に対応するパターンを形成したフォトマスクを介して行うことができる。また、スポット的に紫外線を照射し硬化させる方法等が挙げられる。放射線硬化型の粘着剤層2の形成は、セパレータ上に設けたものを支持基材1上に転写することにより行うことができる。部分的な放射線硬化はセパレータ上に設けた放射線硬化型の粘着剤層2に行うこともできる。   Examples of the method for forming the portion 2a on the pressure-sensitive adhesive layer 2 include a method in which after the radiation-curable pressure-sensitive adhesive layer 2 is formed on the support substrate 1, the portion 2a is partially irradiated with radiation to be cured. It is done. The partial radiation irradiation can be performed through a photomask in which a pattern corresponding to the portion 3b other than the workpiece pasting portion 3a is formed. Moreover, the method etc. of irradiating and hardening | curing an ultraviolet-ray spotly are mentioned. The radiation curable pressure-sensitive adhesive layer 2 can be formed by transferring what is provided on the separator onto the support substrate 1. Partial radiation curing can also be performed on the radiation curable pressure-sensitive adhesive layer 2 provided on the separator.

また、粘着剤層2を放射線硬化型粘着剤により形成する場合には、支持基材1の少なくとも片面の、ワーク貼り付け部分3aに対応する部分以外の部分の全部又は一部が遮光されたものを用い、これに放射線硬化型の粘着剤層2を形成した後に放射線照射して、ワーク貼り付け部分3aに対応する部分を硬化させ、粘着力を低下させた前記部分2aを形成することができる。遮光材料としては、支持フィルム上でフォトマスクになりえるものを印刷や蒸着等で作成することができる。かかる製造方法によれば、効率よく本発明のダイシングシート付きダイボンドフィルム10を製造可能である。   In the case where the pressure-sensitive adhesive layer 2 is formed of a radiation curable pressure-sensitive adhesive, all or a part of at least one side of the support substrate 1 other than the part corresponding to the workpiece pasting part 3a is shielded from light. The portion 2a with reduced adhesive strength can be formed by irradiating with radiation after forming the radiation-curable pressure-sensitive adhesive layer 2 on the substrate and curing the portion corresponding to the workpiece pasting portion 3a. . As a light shielding material, what can become a photomask on a support film can be prepared by printing, vapor deposition, or the like. According to this manufacturing method, the die-bonding film 10 with a dicing sheet of this invention can be manufactured efficiently.

なお、放射線照射の際に、酸素による硬化阻害が起こる場合は、放射線硬化型の粘着剤層2の表面よりなんらかの方法で酸素(空気)を遮断するのが望ましい。例えば、前記粘着剤層2の表面をセパレータで被覆する方法や、窒素ガス雰囲気中で紫外線等の放射線の照射を行う方法等が挙げられる。   In addition, when curing inhibition by oxygen occurs during irradiation, it is desirable to block oxygen (air) from the surface of the radiation curable pressure-sensitive adhesive layer 2 by some method. For example, a method of coating the surface of the pressure-sensitive adhesive layer 2 with a separator, a method of irradiating ultraviolet rays or the like in a nitrogen gas atmosphere, and the like can be mentioned.

粘着剤層2の厚さは、特に限定されないが、チップ切断面の欠け防止や接着層の固定保持の両立性等の点よりは、1〜50μm程度であるのが好ましい。好ましくは2〜30μm、さらには5〜25μmが好ましい。   The thickness of the pressure-sensitive adhesive layer 2 is not particularly limited, but is preferably about 1 to 50 μm from the viewpoint of preventing chipping of the chip cut surface and compatibility of fixing and holding the adhesive layer. Preferably it is 2-30 micrometers, Furthermore, 5-25 micrometers is preferable.

ダイボンドフィルム3、3’は、熱硬化後の熱伝導率が1W/m・K以上であり、1.2W/m・K以上であることが好ましく、1.5W/m・K以上であることがより好ましい。熱硬化後の熱伝導率が1W/m・K以上であるため、ダイボンドフィルム3、3’を用いて製造される半導体装置は、放熱性に優れる。なお、ダイボンドフィルム3、3’の熱硬化後の熱伝導率は高いほど好ましいが、例えば、20W/m・K以下である。
本発明において、「熱硬化後の熱伝導率」とは、130℃で1時間加熱し、続いて、175℃で5時間加熱した後の熱伝導率をいう。
The die bond films 3 and 3 ′ have a thermal conductivity of 1 W / m · K or more after thermosetting, preferably 1.2 W / m · K or more, and 1.5 W / m · K or more. Is more preferable. Since the thermal conductivity after thermosetting is 1 W / m · K or more, the semiconductor device manufactured using the die bond films 3 and 3 ′ is excellent in heat dissipation. In addition, although the heat conductivity after thermosetting of die-bonding films 3 and 3 'is so preferable that it is high, it is 20 W / m * K or less, for example.
In the present invention, “thermal conductivity after thermosetting” refers to the thermal conductivity after heating at 130 ° C. for 1 hour and then heating at 175 ° C. for 5 hours.

また、ダイボンドフィルム3、3’は、130℃において、ずり速度50(1/秒)で測定される溶融粘度が200Pa・s以下であり、好ましくは1〜200Pa・sの範囲内であり、より好ましくは、20〜185Pa・sの範囲内である。130℃において、ずり速度50(1/秒)で測定される溶融粘度、すなわち、130℃における高速せん断時の溶融粘度が200Pa・s以下であるため、ダイボンドフィルム3、3’を被着体に貼り付ける際の圧力により、熱硬化型ダイボンドフィルムの粘度が低下する。従って、プリント配線基板などの被着体の凹凸に十分に追従でき、ボイドの発生を抑制することができる。   The die bond films 3 and 3 ′ have a melt viscosity of 200 Pa · s or less, preferably in the range of 1 to 200 Pa · s, measured at a shear rate of 50 (1 / second) at 130 ° C., more Preferably, it is in the range of 20 to 185 Pa · s. Since the melt viscosity measured at a shear rate of 50 (1 / second) at 130 ° C., that is, the melt viscosity at high shear at 130 ° C. is 200 Pa · s or less, the die bond films 3 and 3 ′ are attached to the adherend. The viscosity of the thermosetting die-bonding film decreases due to the pressure applied. Accordingly, it is possible to sufficiently follow the unevenness of the adherend such as a printed wiring board and to suppress the generation of voids.

また、ダイボンドフィルム3、3’は、ずり速度5(1/秒)で測定される130℃における溶融粘度が10Pa・s〜300Pa・sの範囲内であり、20Pa・s〜280Pa・sの範囲内であること好ましく、50Pa・s〜250Pa・sの範囲内であることがより好ましい。ずり速度5(1/秒)で測定される130℃における溶融粘度が10Pa・s〜300Pa・sの範囲内であるため、フィルムの形状を維持しつつも、比較的低粘度である。従って、プリント配線基板などの被着体の凹凸に十分に追従でき、ボイドの発生を抑制することができる。   The die bond films 3, 3 ′ have a melt viscosity at 130 ° C. measured at a shear rate of 5 (1 / second) within a range of 10 Pa · s to 300 Pa · s, and within a range of 20 Pa · s to 280 Pa · s. Preferably, it is within the range of 50 Pa · s to 250 Pa · s. Since the melt viscosity at 130 ° C. measured at a shear rate of 5 (1 / second) is within the range of 10 Pa · s to 300 Pa · s, the viscosity is relatively low while maintaining the shape of the film. Accordingly, it is possible to sufficiently follow the unevenness of the adherend such as a printed wiring board and to suppress the generation of voids.

また、ダイボンドフィルム3、3’は、熱伝導率が12W/m・K以上の熱伝導性粒子を、熱硬化型ダイボンドフィルム全体に対して75重量%以上含有しており、80重量%以上含有することが好ましく、85重量%以上含有することがより好ましい。また、前記熱伝導性粒子の含有量は、多いほどが好ましいが製膜性の観点から、例えば、93重量%以下である。熱伝導率が12W/m・K以上の熱伝導性粒子を、熱硬化型ダイボンドフィルム全体に対して75重量%以上含有するため、当該熱硬化型ダイボンドフィルムを用いて製造される半導体装置は、より放熱性に優れる。なお、熱伝導性粒子の熱伝導率は、X線構造解析によって得られた熱伝導性粒子の結晶構造から推定できる。   In addition, the die bond films 3 and 3 ′ contain 75% by weight or more and 80% by weight or more of thermally conductive particles having a thermal conductivity of 12 W / m · K or more with respect to the entire thermosetting die bond film. The content is preferably 85% by weight or more. The content of the heat conductive particles is preferably as much as possible, but is 93% by weight or less, for example, from the viewpoint of film forming properties. In order to contain 75% by weight or more of thermally conductive particles having a thermal conductivity of 12 W / m · K or more with respect to the entire thermosetting die bond film, a semiconductor device manufactured using the thermosetting die bond film is: Excellent heat dissipation. The thermal conductivity of the thermally conductive particles can be estimated from the crystal structure of the thermally conductive particles obtained by X-ray structural analysis.

前記熱伝導性粒子は、アルミナ粒子(熱伝導率:36W/m・K)、酸化亜鉛粒子(熱伝導率:54W/m・K)、窒化アルミニウム粒子(熱伝導率:150W/m・K)、窒化ケイ素粒子(熱伝導率:27W/m・K)、炭化ケイ素粒子(熱伝導率:200W/m・K)、酸化マグネシウム粒子(熱伝導率:59W/m・K)、及び、窒化ホウ素粒子(熱伝導率:60W/m・K)からなる群より選択される少なくとも1種の粒子であることが好ましい。特にアルミナは高熱伝導率であり、分散性、入手容易性の点で好ましい。また、窒化ホウ素はさらに高い熱伝導率があることから、好適に用いることができる。   The thermally conductive particles are alumina particles (thermal conductivity: 36 W / m · K), zinc oxide particles (thermal conductivity: 54 W / m · K), aluminum nitride particles (thermal conductivity: 150 W / m · K). Silicon nitride particles (thermal conductivity: 27 W / m · K), silicon carbide particles (thermal conductivity: 200 W / m · K), magnesium oxide particles (thermal conductivity: 59 W / m · K), and boron nitride It is preferably at least one kind of particles selected from the group consisting of particles (thermal conductivity: 60 W / m · K). In particular, alumina has a high thermal conductivity, and is preferable in terms of dispersibility and availability. Boron nitride can be preferably used because of its higher thermal conductivity.

熱伝導性粒子は、シランカップリング剤により処理(前処理)されたものが好ましい。これにより、熱伝導性粒子の分散性が良好になり、熱伝導性粒子の高充填化が可能になる。   The thermally conductive particles are preferably treated (pretreated) with a silane coupling agent. As a result, the dispersibility of the heat conductive particles becomes good, and the heat conductive particles can be highly filled.

シランカップリング剤としては、ケイ素原子、加水分解性基及び有機官能基を含むものが好ましい。   As the silane coupling agent, those containing a silicon atom, a hydrolyzable group and an organic functional group are preferable.

加水分解性基は、ケイ素原子に結合している。   The hydrolyzable group is bonded to the silicon atom.

加水分解性基としては、例えば、メトキシ基、エトキシ基などが挙げられる。なかでも、加水分解速度が速く処理が容易という理由から、メトキシ基が好ましい。   Examples of the hydrolyzable group include a methoxy group and an ethoxy group. Of these, a methoxy group is preferred because of its high hydrolysis rate and easy treatment.

シランカップリング剤中の加水分解性基の数は、熱伝導性粒子と架橋しつつシランカップリング剤同士で架橋することが可能で、熱伝導性粒子表面の架橋点が少なくても熱伝導性粒子全体をシランカップリング剤で表面処理できるという点から、好ましくは2〜3個、より好ましくは3個である。   The number of hydrolyzable groups in the silane coupling agent can be cross-linked between the silane coupling agents while cross-linking with the heat conductive particles. From the point that the whole particle can be surface-treated with a silane coupling agent, the number is preferably 2 to 3, more preferably 3.

有機官能基は、ケイ素原子に結合している。   The organic functional group is bonded to the silicon atom.

有機官能基としては、例えば、アクリル基、メタクリル基、エポキシ基、フェニルアミノ基などを含むものが挙げられる。なかでも、エポキシ樹脂と反応性を有さず、処理を行った熱伝導性粒子の保存安定性が良好なことからアクリル基が好ましい。   As an organic functional group, what contains an acryl group, a methacryl group, an epoxy group, a phenylamino group etc. is mentioned, for example. Among them, an acrylic group is preferable because it has no reactivity with the epoxy resin and the storage stability of the thermally conductive particles that have been treated is good.

なお、エポキシ基と反応性が高い官能基を有するとエポキシ樹脂と反応するため、保存安定性、流動性が低下する。流動性の低下を抑制するという点から、有機官能基としては、一級アミノ基、メルカプト基又はイソシアネート基を含まないものが好ましい。   In addition, since it will react with an epoxy resin when it has a functional group with high reactivity with an epoxy group, storage stability and fluidity | liquidity will fall. From the viewpoint of suppressing a decrease in fluidity, the organic functional group preferably does not contain a primary amino group, mercapto group or isocyanate group.

シランカップリング剤中の有機官能基の数は、好ましくは1個である。ケイ素原子は結合を4つつくるため、有機官能基が多いと加水分解基の数が不足する。   The number of organic functional groups in the silane coupling agent is preferably one. Since the silicon atom has four bonds, if the number of organic functional groups is large, the number of hydrolyzable groups is insufficient.

シランカップリング剤は、ケイ素原子に結合するアルキル基をさらに含んでもよい。シランカップリング剤がアルキル基を含むことにより、メタクリル基よりも反応性を低くすることが可能で、急激な反応による表面処理の偏りを防ぐことができる。アルキル基としては、メチル基、ジメチル基などが挙げられる。なかでも、メチル基が好ましい。   The silane coupling agent may further include an alkyl group bonded to the silicon atom. When the silane coupling agent contains an alkyl group, it is possible to make the reactivity lower than that of the methacryl group, and to prevent surface treatment bias due to abrupt reaction. Examples of the alkyl group include a methyl group and a dimethyl group. Of these, a methyl group is preferable.

シランカップリング剤として、具体的には、2−(3,4−エポキシシクロへキシル)エチルトリメトキシシラン、3−グリシドキシプロピルトリメトキシシラン、3−グリシドキシプロピルトリエトキシシラン、3−グリシドキシプロピルメチルジメトキシシラン、3−グリシドキシプロピルメチルジエトキシシラン、ジメチルジメトキシシラン、ジメチルジエトキシシラン、メチルトリメトキシシラン、メチルトリエトキシシラン、フェニルトリメトキシシラン、フェニルトリエトキシシラン、N−フェニル−3−アミノプロピルトリメトキシシラン、3−メタクリロキシプロピルメチルジメトキシシラン、3−メタクリロキシプロピルトリメトキシシラン、3−メタクリロキシプロピルメチルジエトキシシラン、3−メタクリロキシプロピルトリエトキシシランなどが挙げられる。   Specific examples of the silane coupling agent include 2- (3,4-epoxycyclohexyl) ethyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, 3- Glycidoxypropylmethyldimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, dimethyldimethoxysilane, dimethyldiethoxysilane, methyltrimethoxysilane, methyltriethoxysilane, phenyltrimethoxysilane, phenyltriethoxysilane, N- Phenyl-3-aminopropyltrimethoxysilane, 3-methacryloxypropylmethyldimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropylmethyldiethoxysilane, 3-methacryloxyp Such as pills triethoxy silane.

シランカップリング剤により熱伝導性粒子を処理する方法としては特に限定されず、溶媒中で熱伝導性粒子とシランカップリング剤を混合する湿式法、気相中で熱伝導性粒子とシランカップリング剤を処理させる乾式法などが挙げられる。   The method for treating thermally conductive particles with a silane coupling agent is not particularly limited, and is a wet method in which thermally conductive particles and a silane coupling agent are mixed in a solvent, thermally conductive particles and silane coupling in a gas phase. Examples include a dry method in which the agent is treated.

シランカップリング剤の処理量は特に限定されないが、熱伝導性粒子100重量部に対して、シランカップリング剤を0.05〜5重量部処理することが好ましい。   The treatment amount of the silane coupling agent is not particularly limited, but it is preferable to treat 0.05 to 5 parts by weight of the silane coupling agent with respect to 100 parts by weight of the heat conductive particles.

前記熱伝導性粒子の形状としては、特に限定されず、例えば、フレーク状、針状、フィラメント状、球状、鱗片状のものを使用することができるが、分散性、充填率の向上の点で球状のものが好ましい。   The shape of the heat conductive particles is not particularly limited. For example, flakes, needles, filaments, spheres, and scales can be used, but in terms of improving dispersibility and filling rate. A spherical one is preferred.

前記熱伝導性粒子の平均粒径は、1μm以上10μm以下が好ましく、1.5μm以上8μm以下がより好ましい。前記熱伝導性粒子の平均粒径を1μm以上とすることにより、熱硬化型ダイボンドフィルムの被着体への濡れ性を確保して良好な接着性を発揮させることができる。また、前記熱伝導性粒子の平均粒径を1μm以下とすることにより、熱伝導性粒子の添加による熱伝導性の向上効果をより良好なものとすることができる。また、前記熱伝導性粒子の平均粒径を10μm以下とすることにより、熱硬化型ダイボンドフィルムの厚さを薄くすることができ、ひいては半導体チップを高積層化することができると共に、熱硬化型ダイボンドフィルムから熱伝導性粒子が突き出すことによるチップクラックの発生を防止することができる。なお、熱伝導性粒子の平均粒径は、光度式の粒度分布計(HORIBA製、装置名;LA−910)により求めた値である。   The average particle size of the heat conductive particles is preferably 1 μm or more and 10 μm or less, and more preferably 1.5 μm or more and 8 μm or less. By setting the average particle size of the heat conductive particles to 1 μm or more, it is possible to ensure wettability to the adherend of the thermosetting die-bonding film and to exhibit good adhesiveness. Moreover, the thermal conductivity improvement effect by addition of a heat conductive particle can be made more favorable by the average particle diameter of the said heat conductive particle being 1 micrometer or less. Further, by setting the average particle size of the thermally conductive particles to 10 μm or less, the thickness of the thermosetting die-bonding film can be reduced, and as a result, the semiconductor chip can be highly laminated, and the thermosetting type Generation | occurrence | production of the chip crack by heat conductive particle protruding from a die-bonding film can be prevented. The average particle diameter of the thermally conductive particles is a value determined by a photometric particle size distribution meter (manufactured by HORIBA, apparatus name: LA-910).

また、前記熱伝導性粒子としては、平均粒子径の異なる2種以上の熱伝導性粒子を用いてもよい。平均粒径の異なる2種以上の熱伝導性粒子を用いることにより、充填率を向上させ易くすることができるからである。   Further, as the heat conductive particles, two or more kinds of heat conductive particles having different average particle diameters may be used. This is because it is possible to easily improve the filling rate by using two or more kinds of thermally conductive particles having different average particle diameters.

ダイボンドフィルム3、3’の積層構造は特に限定されず、例えば接着剤層の単層のみからなるものや、コア材料の片面又は両面に接着剤層を形成した多層構造のもの等が挙げられる。前記コア材料としては、フィルム(例えばポリイミドフィルム、ポリエステルフィルム、ポリエチレンテレフタレートフィルム、ポリエチレンナフタレートフィルム、ポリカーボネートフィルム等)、ガラス繊維やプラスチック製不織繊維で強化された樹脂基板、シリコン基板又はガラス基板等が挙げられる。   The laminated structure of the die bond films 3 and 3 ′ is not particularly limited, and examples thereof include a single-layer adhesive layer and a multilayer structure in which an adhesive layer is formed on one or both sides of the core material. Examples of the core material include a film (for example, a polyimide film, a polyester film, a polyethylene terephthalate film, a polyethylene naphthalate film, and a polycarbonate film), a resin substrate reinforced with glass fibers or plastic non-woven fibers, a silicon substrate, a glass substrate, or the like. Is mentioned.

ダイボンドフィルム3、3’は、熱可塑性樹脂、熱硬化性樹脂などの樹脂成分を含むことが好ましい。   The die bond films 3 and 3 ′ preferably include a resin component such as a thermoplastic resin and a thermosetting resin.

前記熱硬化性樹脂としては、フェノール樹脂、アミノ樹脂、不飽和ポリエステル樹脂、エポキシ樹脂、ポリウレタン樹脂、シリコーン樹脂、又は熱硬化性ポリイミド樹脂等が挙げられる。これらの樹脂は、単独で又は2種以上を併用して用いることができる。特に、半導体チップを腐食させるイオン性不純物等の含有が少ないエポキシ樹脂が好ましい。また、エポキシ樹脂の硬化剤としてはフェノール樹脂が好ましい。   Examples of the thermosetting resin include phenol resin, amino resin, unsaturated polyester resin, epoxy resin, polyurethane resin, silicone resin, and thermosetting polyimide resin. These resins can be used alone or in combination of two or more. In particular, an epoxy resin containing a small amount of ionic impurities that corrode the semiconductor chip is preferable. Moreover, as a hardening | curing agent of an epoxy resin, a phenol resin is preferable.

前記エポキシ樹脂は、ダイボンド用途の接着剤として一般に用いられるものであれば特に限定は無く、例えばビスフェノールA型、ビスフェノールF型、ビスフェノールS型、臭素化ビスフェノールA型、水添ビスフェノールA型、ビスフェノールAF型、ビフェニル型、ナフタレン型、フルオンレン型、フェノールノボラック型、オルソクレゾールノボラック型、トリスヒドロキシフェニルメタン型、テトラフェニロールエタン型等の二官能エポキシ樹脂や多官能エポキシ樹脂、又はヒダントイン型、トリスグリシジルイソシアヌレート型若しくはグリシジルアミン型等のエポキシ樹脂が用いられる。これらは単独で、又は2種以上を併用して用いることができる。これらのエポキシ樹脂のうちノボラック型エポキシ樹脂、ビフェニル型エポキシ樹脂、トリスヒドロキシフェニルメタン型樹脂又はテトラフェニロールエタン型エポキシ樹脂が特に好ましい。これらのエポキシ樹脂は、硬化剤としてのフェノール樹脂との反応性に富み、耐熱性等に優れるからである。
また、前記エポキシ樹脂は、室温(23℃)で固形のものと、室温(23℃)で液状のものとの2種類を併用して用いることができる。室温で固形のエポキシ樹脂に対して、室温で液状のエポキシ樹脂を加えることにより、フィルムを形成した際の脆弱性を改善することができ、作業性を向上させることができる。
The epoxy resin is not particularly limited as long as it is generally used as an adhesive for die bonding. For example, bisphenol A type, bisphenol F type, bisphenol S type, brominated bisphenol A type, hydrogenated bisphenol A type, bisphenol AF Type, biphenyl type, naphthalene type, fluorene type, phenol novolac type, orthocresol novolak type, trishydroxyphenylmethane type, tetraphenylolethane type, etc., or bifunctional epoxy resin, or hydantoin type, trisglycidyl isocyanate An epoxy resin such as a nurate type or a glycidylamine type is used. These can be used alone or in combination of two or more. Of these epoxy resins, novolac type epoxy resins, biphenyl type epoxy resins, trishydroxyphenylmethane type resins or tetraphenylolethane type epoxy resins are particularly preferred. This is because these epoxy resins are rich in reactivity with a phenol resin as a curing agent and are excellent in heat resistance and the like.
Moreover, the said epoxy resin can be used in combination of 2 types, a solid thing at room temperature (23 degreeC), and a liquid thing at room temperature (23 degreeC). By adding an epoxy resin that is liquid at room temperature to an epoxy resin that is solid at room temperature, the brittleness when forming a film can be improved, and workability can be improved.

更に、前記フェノール樹脂は、前記エポキシ樹脂の硬化剤として作用するものであり、例えば、フェノールノボラック樹脂、フェノールアラルキル樹脂、クレゾールノボラック樹脂、tert−ブチルフェノールノボラック樹脂、ノニルフェノールノボラック樹脂等のノボラック型フェノール樹脂、レゾール型フェノール樹脂、ポリパラオキシスチレン等のポリオキシスチレン等が挙げられる。これらは単独で、又は2種以上を併用して用いることができる。これらのフェノール樹脂のうちフェノールノボラック樹脂、フェノールアラルキル樹脂が特に好ましい。半導体装置の接続信頼性を向上させることができるからである。   Further, the phenol resin acts as a curing agent for the epoxy resin. Examples include resol-type phenolic resins and polyoxystyrenes such as polyparaoxystyrene. These can be used alone or in combination of two or more. Of these phenol resins, phenol novolac resins and phenol aralkyl resins are particularly preferred. This is because the connection reliability of the semiconductor device can be improved.

前記熱硬化性樹脂(例えば、エポキシ樹脂やフェノール樹脂)なかでも、低速せん断応力(例えば、ずり速度5(1/秒))印加下での熱硬化型ダイボンドフィルムの130℃での溶融粘度を低下できる観点から、軟化点が100℃以下のものが好ましい。
また、前記熱硬化性樹脂(例えば、エポキシ樹脂やフェノール樹脂)なかでも、室温で液状のものを含むことが好ましい。複数種類の熱硬化性樹脂を含有させる場合、少なくとも、一種の熱硬化性樹脂が室温で液状であればよい。前記熱硬化性樹脂が、室温で液状のものを含むと、被着体の凹凸により十分に追従でき、ボイドの発生を抑制することができる。
なお、エポキシ樹脂の軟化点は、JIS K 7234−1986に規定される環球法で測定できる。また、フェノール樹脂の軟化点は、JIS K 6910−2007に規定される環球法で測定できる。
Among the thermosetting resins (for example, epoxy resins and phenol resins), the melt viscosity at 130 ° C. of the thermosetting die-bonding film under the application of low shear stress (for example, shear rate 5 (1 / second)) is lowered. From the viewpoint that it can be made, those having a softening point of 100 ° C. or less are preferable.
Further, among the thermosetting resins (for example, epoxy resins and phenol resins), it is preferable to include those that are liquid at room temperature. When multiple types of thermosetting resins are included, at least one type of thermosetting resin may be liquid at room temperature. If the thermosetting resin contains a liquid at room temperature, it can sufficiently follow the unevenness of the adherend, and the generation of voids can be suppressed.
In addition, the softening point of an epoxy resin can be measured by the ring and ball method prescribed | regulated to JISK7234-1986. Moreover, the softening point of a phenol resin can be measured by the ring and ball method prescribed | regulated to JISK6910-2007.

前記エポキシ樹脂とフェノール樹脂との配合割合は、例えば、前記エポキシ樹脂成分中のエポキシ基1当量当たりフェノール樹脂中の水酸基が0.5〜2.0当量になるように配合することが好適である。より好適なのは、0.8〜1.2当量である。即ち、両者の配合割合が前記範囲を外れると、十分な硬化反応が進まず、エポキシ樹脂硬化物の特性が劣化し易くなるからである。   The mixing ratio of the epoxy resin and the phenol resin is preferably such that, for example, the hydroxyl group in the phenol resin is 0.5 to 2.0 equivalents per 1 equivalent of the epoxy group in the epoxy resin component. . More preferred is 0.8 to 1.2 equivalents. That is, if the blending ratio of both is out of the above range, sufficient curing reaction does not proceed and the properties of the cured epoxy resin are likely to deteriorate.

前記熱可塑性樹脂としては、天然ゴム、ブチルゴム、イソプレンゴム、クロロプレンゴム、エチレン−酢酸ビニル共重合体、エチレン−アクリル酸共重合体、エチレン−アクリル酸エステル共重合体、ポリブタジエン樹脂、ポリカーボネート樹脂、熱可塑性ポリイミド樹脂、6−ナイロンや6,6−ナイロン等のポリアミド樹脂、フェノキシ樹脂、アクリル樹脂、PETやPBT等の飽和ポリエステル樹脂、ポリアミドイミド樹脂、又はフッ素樹脂等が挙げられる。これらの熱可塑性樹脂は単独で、又は2種以上を併用して用いることができる。これらの熱可塑性樹脂のうち、イオン性不純物が少なく耐熱性が高く、半導体チップの信頼性を確保できるアクリル樹脂が特に好ましい。   Examples of the thermoplastic resin include natural rubber, butyl rubber, isoprene rubber, chloroprene rubber, ethylene-vinyl acetate copolymer, ethylene-acrylic acid copolymer, ethylene-acrylic acid ester copolymer, polybutadiene resin, polycarbonate resin, heat Examples thereof include plastic polyimide resins, polyamide resins such as 6-nylon and 6,6-nylon, phenoxy resins, acrylic resins, saturated polyester resins such as PET and PBT, polyamideimide resins, and fluorine resins. These thermoplastic resins can be used alone or in combination of two or more. Among these thermoplastic resins, an acrylic resin that has few ionic impurities and high heat resistance and can ensure the reliability of the semiconductor chip is particularly preferable.

前記アクリル樹脂としては、特に限定されるものではなく、炭素数30以下、特に炭素数4〜18の直鎖若しくは分岐のアルキル基を有するアクリル酸又はメタクリル酸のエステルの1種又は2種以上を成分とする重合体(アクリル共重合体)等が挙げられる。前記アルキル基としては、例えばメチル基、エチル基、プロピル基、イソプロピル基、n−ブチル基、t−ブチル基、イソブチル基、アミル基、イソアミル基、ヘキシル基、へプチル基、シクロヘキシル基、2−エチルヘキシル基、オクチル基、イソオクチル基、ノニル基、イソノニル基、デシル基、イソデシル基、ウンデシル基、ラウリル基、トリデシル基、テトラデシル基、ステアリル基、オクタデシル基、又はドデシル基等が挙げられる。   The acrylic resin is not particularly limited, and includes one or two or more esters of acrylic acid or methacrylic acid having a linear or branched alkyl group having 30 or less carbon atoms, particularly 4 to 18 carbon atoms. Examples thereof include a polymer (acrylic copolymer) as a component. Examples of the alkyl group include a methyl group, ethyl group, propyl group, isopropyl group, n-butyl group, t-butyl group, isobutyl group, amyl group, isoamyl group, hexyl group, heptyl group, cyclohexyl group, 2- Examples include an ethylhexyl group, an octyl group, an isooctyl group, a nonyl group, an isononyl group, a decyl group, an isodecyl group, an undecyl group, a lauryl group, a tridecyl group, a tetradecyl group, a stearyl group, an octadecyl group, and a dodecyl group.

また、前記重合体を形成する他のモノマーとしては、特に限定されるものではなく、例えばアクリル酸、メタクリル酸、カルボキシエチルアクリレート、カルボキシペンチルアクリレート、イタコン酸、マレイン酸、フマール酸若しくはクロトン酸等の様なカルボキシル基含有モノマー、無水マレイン酸若しくは無水イタコン酸等の様な酸無水物モノマー、(メタ)アクリル酸2−ヒドロキシエチル、(メタ)アクリル酸2−ヒドロキシプロピル、(メタ)アクリル酸4−ヒドロキシブチル、(メタ)アクリル酸6−ヒドロキシヘキシル、(メタ)アクリル酸8−ヒドロキシオクチル、(メタ)アクリル酸10−ヒドロキシデシル、(メタ)アクリル酸12−ヒドロキシラウリル若しくは(4−ヒドロキシメチルシクロヘキシル)−メチルアクリレート等の様なヒドロキシル基含有モノマー、スチレンスルホン酸、アリルスルホン酸、2−(メタ)アクリルアミド−2−メチルプロパンスルホン酸、(メタ)アクリルアミドプロパンスルホン酸、スルホプロピル(メタ)アクリレート若しくは(メタ)アクリロイルオキシナフタレンスルホン酸等の様なスルホン酸基含有モノマー、又は2−ヒドロキシエチルアクリロイルホスフェート等の様な燐酸基含有モノマーが挙げられる。   In addition, the other monomer forming the polymer is not particularly limited, and examples thereof include acrylic acid, methacrylic acid, carboxyethyl acrylate, carboxypentyl acrylate, itaconic acid, maleic acid, fumaric acid, and crotonic acid. Carboxyl group-containing monomers such as acid anhydride monomers such as maleic anhydride or itaconic anhydride, 2-hydroxyethyl (meth) acrylate, 2-hydroxypropyl (meth) acrylate, 4- (meth) acrylic acid 4- Hydroxybutyl, 6-hydroxyhexyl (meth) acrylate, 8-hydroxyoctyl (meth) acrylate, 10-hydroxydecyl (meth) acrylate, 12-hydroxylauryl (meth) acrylate or (4-hydroxymethylcyclohexyl) -Methyla Hydroxyl group-containing monomers such as relate, styrene sulfonic acid, allyl sulfonic acid, 2- (meth) acrylamide-2-methylpropane sulfonic acid, (meth) acrylamide propane sulfonic acid, sulfopropyl (meth) acrylate or (meth) Examples thereof include sulfonic acid group-containing monomers such as acryloyloxynaphthalene sulfonic acid, and phosphoric acid group-containing monomers such as 2-hydroxyethylacryloyl phosphate.

前記熱硬化性樹脂と前記熱可塑性樹脂の配合割合としては、前記熱硬化性樹脂の含有重量部をAとし、前記熱可塑性樹脂の含有重量部をBとしたときに、A/Bが5以上であることが好ましく、7以上であることがより好ましく9以上であることがさらに好ましい。なお、本明細書では、熱硬化性樹脂の分子量は5000未満であり、熱可塑性樹脂の分子量は5000以上である。   As a blending ratio of the thermosetting resin and the thermoplastic resin, A / B is 5 or more when the content part by weight of the thermosetting resin is A and the content part by weight of the thermoplastic resin is B. Preferably, it is 7 or more, more preferably 9 or more. In addition, in this specification, the molecular weight of a thermosetting resin is less than 5000, and the molecular weight of a thermoplastic resin is 5000 or more.

樹脂成分の含有量は、ダイボンドフィルム3、3’全体に対して、好ましくは7重量%以上である。樹脂成分の含有量は、ダイボンドフィルム3、3’全体に対して好ましくは25重量%以下、より好ましくは20重量%以下、さらに好ましくは15重量%以下である。   The content of the resin component is preferably 7% by weight or more with respect to the entire die-bonding films 3, 3 '. The content of the resin component is preferably 25% by weight or less, more preferably 20% by weight or less, and still more preferably 15% by weight or less with respect to the entire die bond film 3, 3 '.

樹脂成分(熱硬化性樹脂と熱可塑性樹脂の合計量)中の熱硬化性樹脂の配合割合としては、所定条件下で加熱した際にダイボンドフィルム3、3’が熱硬化型としての機能を発揮する程度であれば特に限定されないが、130℃における低速せん断時(ずり速度5(1/秒))の溶融粘度を低くするために、75〜99重量%の範囲内であることが好ましく、85〜98重量%の範囲内であることがより好ましい。   As a compounding ratio of the thermosetting resin in the resin component (total amount of the thermosetting resin and the thermoplastic resin), the die-bonding films 3 and 3 ′ exhibit a function as a thermosetting type when heated under predetermined conditions. In order to reduce the melt viscosity at low shear (shear rate 5 (1 / sec)) at 130 ° C., it is preferably in the range of 75 to 99% by weight. More preferably, it is in the range of -98% by weight.

また、樹脂成分中の熱可塑性樹脂の配合割合としては、130℃における低速せん断時(ずり速度5(1/秒))の溶融粘度を低くするために、1〜25重量%の範囲内であることが好ましく、2〜15重量%の範囲内であることがより好ましい。   Further, the blending ratio of the thermoplastic resin in the resin component is in the range of 1 to 25% by weight in order to reduce the melt viscosity at low shear (shear rate 5 (1 / second)) at 130 ° C. It is preferable that it is in the range of 2 to 15% by weight.

ダイボンドフィルム3、3’は硬化触媒を含むことが好ましい。これにより、エポキシ樹脂とフェノール樹脂等の硬化剤との熱硬化を促進できる。硬化触媒としては特に限定されないが、例えば、テトラフェニルホスホニウムテトラフェニルボレート(商品名;TPP−K)、テトラフェニルホスホニウムテトラ−p−トリボレート(商品名;TPP−MK)、トリフェニルホスフィントリフェニルボラン(商品名;TPP−S)などのリン−ホウ素系硬化触媒が挙げられる(いずれも北興化学工業(株)製)。なかでも、潜在性に優れるため室温での保存安定性が良好であるという点から、テトラフェニルホスホニウムテトラ−p−トリボレートが好ましい。   The die bond films 3, 3 'preferably include a curing catalyst. Thereby, thermal curing with a curing agent such as an epoxy resin and a phenol resin can be promoted. Although it does not specifically limit as a curing catalyst, For example, tetraphenylphosphonium tetraphenylborate (brand name; TPP-K), tetraphenylphosphonium tetra-p-triborate (brand name; TPP-MK), triphenylphosphine triphenylborane ( Examples thereof include phosphorus-boron curing catalysts such as trade name: TPP-S (all manufactured by Hokuko Chemical Co., Ltd.). Among these, tetraphenylphosphonium tetra-p-triborate is preferable from the viewpoint that it has excellent latency and thus has good storage stability at room temperature.

硬化触媒の含有量は適宜設定できるが、熱硬化性樹脂100重量部に対して、0.1〜3重量部が好ましく、0.5〜2重量部がより好ましい。   Although content of a curing catalyst can be set suitably, 0.1-3 weight part is preferable with respect to 100 weight part of thermosetting resins, and 0.5-2 weight part is more preferable.

本発明のダイボンドフィルム3、3’を予めある程度架橋をさせておく場合には、作製に際し、重合体の分子鎖末端の官能基等と反応する多官能性化合物を架橋剤として添加させておくのがよい。これにより、高温下での接着特性を向上させ、耐熱性の改善を図ることができる。   When the die-bonding films 3, 3 ′ of the present invention are previously crosslinked to some extent, a polyfunctional compound that reacts with the functional group at the molecular chain end of the polymer is added as a crosslinking agent during production. Is good. Thereby, the adhesive property under high temperature can be improved and heat resistance can be improved.

前記架橋剤としては、従来公知のものを採用することができる。特に、トリレンジイソシアネート、ジフェニルメタンジイソシアネート、p−フェニレンジイソシアネート、1,5−ナフタレンジイソシアネート、多価アルコールとジイソシアネートの付加物等のポリイソシアネート化合物がより好ましい。架橋剤の添加量としては、前記の重合体100重量部に対し、通常0.05〜7重量部とするのが好ましい。架橋剤の量が7重量部より多いと、接着力が低下するので好ましくない。その一方、0.05重量部より少ないと、凝集力が不足するので好ましくない。また、この様なポリイソシアネート化合物と共に、必要に応じて、エポキシ樹脂等の他の多官能性化合物を一緒に含ませるようにしてもよい。   A conventionally well-known thing can be employ | adopted as said crosslinking agent. In particular, polyisocyanate compounds such as tolylene diisocyanate, diphenylmethane diisocyanate, p-phenylene diisocyanate, 1,5-naphthalene diisocyanate, adducts of polyhydric alcohol and diisocyanate are more preferable. The addition amount of the crosslinking agent is usually preferably 0.05 to 7 parts by weight with respect to 100 parts by weight of the polymer. When the amount of the cross-linking agent is more than 7 parts by weight, the adhesive force is lowered, which is not preferable. On the other hand, if it is less than 0.05 parts by weight, the cohesive force is insufficient, which is not preferable. Moreover, you may make it include other polyfunctional compounds, such as an epoxy resin, together with such a polyisocyanate compound as needed.

また、ダイボンドフィルム3、3’には、その用途に応じて前記熱伝導性粒子以外のフィラーを適宜配合することができる。前記フィラーの配合は、弾性率の調節等を可能とする。前記フィラーとしては、無機フィラー、及び、有機フィラーが挙げられる。前記無機フィラーとしては、特に制限はなく、例えば、炭酸カルシウム、炭酸マグネシウム、ケイ酸カルシウム、ケイ酸マグネシウム、酸化カルシウム、ほう酸アルミウィスカ、結晶質シリカ、非晶質シリカ等が挙げられる。これらは、単独で又は2種以上を併用して用いることができる。   Moreover, fillers other than the said heat conductive particle can be suitably mix | blended with the die-bonding films 3 and 3 'according to the use. The blending of the filler enables adjustment of the elastic modulus. Examples of the filler include inorganic fillers and organic fillers. The inorganic filler is not particularly limited, and examples thereof include calcium carbonate, magnesium carbonate, calcium silicate, magnesium silicate, calcium oxide, aluminum borate whisker, crystalline silica, and amorphous silica. These can be used alone or in combination of two or more.

なお、ダイボンドフィルム3、3’には、前記フィラー以外に、必要に応じて他の添加剤を適宜に配合することができる。他の添加剤としては、例えば難燃剤、シランカップリング剤又はイオントラップ剤等が挙げられる。前記難燃剤としては、例えば、三酸化アンチモン、五酸化アンチモン、臭素化エポキシ樹脂等が挙げられる。これらは、単独で、又は2種以上を併用して用いることができる。前記シランカップリング剤としては、例えば、β−(3、4−エポキシシクロヘキシル)エチルトリメトキシシラン、γ−グリシドキシプロピルトリメトキシシラン、γ−グリシドキシプロピルメチルジエトキシシラン等が挙げられる。これらの化合物は、単独で又は2種以上を併用して用いることができる。前記イオントラップ剤としては、例えばハイドロタルサイト類、水酸化ビスマス等が挙げられる。これらは、単独で又は2種以上を併用して用いることができる。   In addition to the said filler, other additives can be suitably mix | blended with the die-bonding films 3 and 3 'as needed. Examples of other additives include flame retardants, silane coupling agents, ion trapping agents, and the like. Examples of the flame retardant include antimony trioxide, antimony pentoxide, brominated epoxy resin, and the like. These can be used alone or in combination of two or more. Examples of the silane coupling agent include β- (3,4-epoxycyclohexyl) ethyltrimethoxysilane, γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropylmethyldiethoxysilane, and the like. These compounds can be used alone or in combination of two or more. Examples of the ion trapping agent include hydrotalcites and bismuth hydroxide. These can be used alone or in combination of two or more.

ダイボンドフィルム3、3’の厚さ(積層体の場合は、総厚)は特に限定されないが、チップ切断面の欠け防止や接着層による固定保持の両立性の観点から、1〜200μmが好ましく、より好ましくは3〜100μm、さらに好ましくは5〜80μmである。   The thickness of the die bond films 3 and 3 ′ (total thickness in the case of a laminate) is not particularly limited, but is preferably 1 to 200 μm from the viewpoint of chipping prevention of chip cut surfaces and compatibility of fixing and holding by an adhesive layer. More preferably, it is 3-100 micrometers, More preferably, it is 5-80 micrometers.

前記ダイシングシート付きダイボンドフィルム10、12は、基材1や粘着剤層、ダイボンドフィルムに対して、その接着時及び剥離時等における静電気の発生やそれによる半導体ウェハ等の帯電で回路が破壊されること等を防止する目的で帯電防止機能を持たせることができる。帯電防止機能の付与は、基材1や粘着剤層2、ダイボンドフィルム3、3’に帯電防止剤や導電性物質の添加する方法、基材1への電荷移動錯体や金属膜等からなる導電層の付設等、適宜な方式で行うことができる。これら方式は半導体ウェハを変質させるおそれのある不純物イオンが発生しにくい方式が好ましい。導電性の付与、導電性の向上等を目的として配合される導電性物質(導電フィラー)としては、銀、アルミニウム、金、銅、ニッケル、導電性合金等の球状、針状、フレーク状の金属粉、アモルファスカーボンブラック、グラファイト等が挙げられる。   The die-bonding films 10 and 12 with the dicing sheet have their circuits destroyed due to the generation of static electricity when the substrate 1, the pressure-sensitive adhesive layer, and the die-bonding film are bonded or peeled off, and charging of the semiconductor wafer or the like. In order to prevent this, an antistatic function can be provided. The antistatic function is imparted by a method of adding an antistatic agent or a conductive substance to the base material 1, the pressure-sensitive adhesive layer 2, or the die bond films 3, 3 ′, a conductive material comprising a charge transfer complex or a metal film to the base material 1. It can be performed by an appropriate method such as attachment of a layer. These systems are preferably systems that do not easily generate impurity ions that may alter the semiconductor wafer. Examples of the conductive substance (conductive filler) blended for the purpose of imparting conductivity and improving conductivity include spherical, acicular, and flaky metals such as silver, aluminum, gold, copper, nickel, and conductive alloys. Examples thereof include powder, amorphous carbon black, and graphite.

前記ダイシングシート付きダイボンドフィルム10、12のダイボンドフィルム3、3’は、セパレータにより保護されていることが好ましい(図示せず)。セパレータは、実用に供するまでダイボンドフィルム3、3’を保護する保護材としての機能を有している。また、セパレータは、さらに、粘着剤層2にダイボンドフィルム3、3’を転写する際の支持基材として用いることができる。セパレータはダイシングシート付きダイボンドフィルムのダイボンドフィルム3、3’上にワークを貼着する際に剥がされる。セパレータとしては、ポリエチレンテレフタレート(PET)、ポリエチレン、ポリプロピレンや、フッ素系剥離剤、長鎖アルキルアクリレート系剥離剤等の剥離剤により表面コートされたプラスチックフィルムや紙等も使用可能である。   It is preferable that the die bond films 3 and 3 ′ of the die bond films 10 and 12 with the dicing sheet are protected by a separator (not shown). The separator has a function as a protective material for protecting the die bond films 3 and 3 ′ until they are put into practical use. Further, the separator can be used as a support base material when transferring the die bond films 3 and 3 ′ to the pressure-sensitive adhesive layer 2. The separator is peeled off when a workpiece is stuck on the die bond film 3, 3 'of the die bond film with a dicing sheet. As the separator, a plastic film or paper surface-coated with a release agent such as polyethylene terephthalate (PET), polyethylene, polypropylene, a fluorine release agent, or a long-chain alkyl acrylate release agent can be used.

本実施の形態に係るダイシングシート付きダイボンドフィルム10、12は、例えば、次の通りにして作製される。
まず、基材1は、従来公知の製膜方法により製膜することができる。当該製膜方法としては、例えばカレンダー製膜法、有機溶媒中でのキャスティング法、密閉系でのインフレーション押出法、Tダイ押出法、共押出し法、ドライラミネート法等が例示できる。
The die-bonding films 10 and 12 with a dicing sheet concerning this Embodiment are produced as follows, for example.
First, the base material 1 can be formed by a conventionally known film forming method. Examples of the film forming method include a calendar film forming method, a casting method in an organic solvent, an inflation extrusion method in a closed system, a T-die extrusion method, a co-extrusion method, and a dry lamination method.

次に、基材1上に粘着剤組成物溶液を塗布して塗布膜を形成した後、該塗布膜を所定条件下で乾燥させ(必要に応じて加熱架橋させて)、粘着剤層2を形成する。塗布方法としては特に限定されず、例えば、ロール塗工、スクリーン塗工、グラビア塗工等が挙げられる。また、乾燥条件としては、例えば乾燥温度80〜150℃、乾燥時間0.5〜5分間の範囲内で行われる。また、セパレータ上に粘着剤組成物を塗布して塗布膜を形成した後、前記乾燥条件で塗布膜を乾燥させて粘着剤層2を形成してもよい。その後、基材1上に粘着剤層2をセパレータと共に貼り合わせる。これにより、ダイシングシート11が作製される。   Next, after a pressure-sensitive adhesive composition solution is applied onto the substrate 1 to form a coating film, the coating film is dried under predetermined conditions (heat-crosslinked as necessary), and the pressure-sensitive adhesive layer 2 is formed. Form. It does not specifically limit as a coating method, For example, roll coating, screen coating, gravure coating, etc. are mentioned. As drying conditions, for example, the drying temperature is 80 to 150 ° C. and the drying time is 0.5 to 5 minutes. Moreover, after apply | coating an adhesive composition on a separator and forming a coating film, the coating film may be dried on the said drying conditions, and the adhesive layer 2 may be formed. Then, the adhesive layer 2 is bonded together with the separator on the base material 1. Thereby, the dicing sheet 11 is produced.

ダイボンドフィルム3、3’は、例えば、次の通りにして作製される。
まず、ダイボンドフィルム3、3’の形成材料である接着剤組成物を作製する。当該接着剤組成物には、前述の通り、必要に応じて、熱可塑性樹脂と、熱可塑性樹脂と、熱伝導性粒子と、その他各種の添加剤等とが配合されている。通常、接着剤組成物は、溶媒に溶解させた溶液状態又は溶媒に分散させた分散液状態で用いられる(以下、溶液状態には分散液状態も含むこととする)。
The die bond films 3 and 3 ′ are produced, for example, as follows.
First, an adhesive composition that is a material for forming the die bond films 3 and 3 ′ is prepared. As described above, the adhesive composition contains a thermoplastic resin, a thermoplastic resin, thermally conductive particles, and other various additives as necessary. Usually, the adhesive composition is used in a solution state dissolved in a solvent or a dispersion state dispersed in a solvent (hereinafter, the solution state includes a dispersion state).

次に、接着剤組成物溶液を基材セパレータ上に所定厚さとなる様に塗布して塗布膜を形成した後、該塗布膜を所定条件下で乾燥させ、接着剤層を形成する。塗布方法としては特に限定されず、例えば、ロール塗工、スクリーン塗工、グラビア塗工等が挙げられる。また、乾燥条件としては、例えば乾燥温度70〜160℃、乾燥時間1〜5分間の範囲内で行われる。また、セパレータ上に粘着剤組成物溶液を塗布して塗布膜を形成した後、前記乾燥条件で塗布膜を乾燥させて接着剤層を形成してもよい。その後、基材セパレータ上に接着剤層をセパレータと共に貼り合わせる。   Next, the adhesive composition solution is applied on the base separator to a predetermined thickness to form a coating film, and then the coating film is dried under predetermined conditions to form an adhesive layer. It does not specifically limit as a coating method, For example, roll coating, screen coating, gravure coating, etc. are mentioned. As drying conditions, for example, the drying temperature is 70 to 160 ° C. and the drying time is 1 to 5 minutes. Moreover, after apply | coating an adhesive composition solution on a separator and forming a coating film, you may dry an application film on the said drying conditions, and may form an adhesive bond layer. Then, an adhesive bond layer is bonded together with a separator on a base material separator.

続いて、ダイシングシート11及び接着剤層からそれぞれセパレータを剥離し、接着剤層と粘着剤層とが貼り合わせ面となる様にして両者を貼り合わせる。貼り合わせは、例えば圧着により行うことができる。このとき、ラミネート温度は特に限定されず、例えば30〜50℃が好ましく、35〜45℃がより好ましい。また、線圧は特に限定されず、例えば0.1〜20kgf/cmが好ましく、1〜10kgf/cmがより好ましい。次に、接着剤層上の基材セパレータを剥離し、本実施の形態に係るダイシングシート付きダイボンドフィルム10、12が得られる。   Subsequently, the separator is peeled off from each of the dicing sheet 11 and the adhesive layer, and the two are bonded together so that the adhesive layer and the pressure-sensitive adhesive layer become a bonding surface. Bonding can be performed by, for example, pressure bonding. At this time, the lamination temperature is not particularly limited, and is preferably 30 to 50 ° C., for example, and more preferably 35 to 45 ° C. Moreover, a linear pressure is not specifically limited, For example, 0.1-20 kgf / cm is preferable and 1-10 kgf / cm is more preferable. Next, the base material separator on the adhesive layer is peeled off, and the die bond films with dicing sheets 10 and 12 according to the present embodiment are obtained.

(半導体装置の製造方法)
本実施形態に係る半導体装置の製造方法は、前記熱硬化型ダイボンドフィルムを準備する工程と、
前記熱硬化型ダイボンドフィルムを介して、半導体チップを被着体上にダイボンドするダイボンド工程とを含む(以下、第1実施形態ともいう)。
また、本実施形態に係る半導体装置の製造方法は、前記に記載のダイシングシート付きダイボンドフィルムを準備する工程と、
前記ダイシングシート付きダイボンドフィルムの熱硬化型ダイボンドフィルムと、半導体ウェハの裏面とを貼り合わせる貼り合わせ工程と、
前記半導体ウェハを前記熱硬化型ダイボンドフィルムと共にダイシングして、チップ状の半導体チップを形成するダイシング工程と、
前記半導体チップを、前記ダイシングシート付きダイボンドフィルムから前記熱硬化型ダイボンドフィルムと共にピックアップするピックアップ工程と、
前記熱硬化型ダイボンドフィルムを介して、前記半導体チップを被着体上にダイボンドするダイボンド工程とを含むものでもある(以下、第2実施形態ともいう)。
第1実施形態に係る半導体装置の製造方法は、第2の実施形態に係る半導体装置の製造方法が、ダイシングシート付きダイボンドフィルムを用いているのに対して、第1実施形態に係る半導体装置の製造方法では、ダイボンドフィルムを単体で用いている点で異なりその他の点で共通する。第1の実施形態に係る半導体装置の製造方法においては、ダイボンドフィルムを準備した後、これをダイシングシートと貼り合わせる工程を行なえば、その後は、第2実施形態に係る半導体装置の製造方法と同様とすることができる。そこで、以下では、第2実施形態に係る半導体装置の製造方法について説明することとする。
(Method for manufacturing semiconductor device)
The method for manufacturing a semiconductor device according to this embodiment includes a step of preparing the thermosetting die bond film,
A die-bonding step of die-bonding a semiconductor chip on an adherend via the thermosetting die-bonding film (hereinafter also referred to as a first embodiment).
Moreover, the method of manufacturing a semiconductor device according to the present embodiment includes a step of preparing the die bond film with a dicing sheet described above,
A bonding step of bonding the thermosetting die-bonding film of the die-bonding film with the dicing sheet and the back surface of the semiconductor wafer;
Dicing the semiconductor wafer together with the thermosetting die bond film to form a chip-shaped semiconductor chip;
A pick-up step of picking up the semiconductor chip together with the thermosetting die-bonding film from the die-bonding film with the dicing sheet;
A die-bonding step of die-bonding the semiconductor chip on an adherend through the thermosetting die-bonding film (hereinafter also referred to as a second embodiment).
The semiconductor device manufacturing method according to the first embodiment is different from the semiconductor device manufacturing method according to the second embodiment in that the die bonding film with a dicing sheet is used. The manufacturing method is different in that the die bond film is used alone, and is common in other points. In the method for manufacturing a semiconductor device according to the first embodiment, after preparing a die bond film and performing a step of bonding it to a dicing sheet, thereafter, the method is the same as the method for manufacturing a semiconductor device according to the second embodiment. It can be. Therefore, hereinafter, a method for manufacturing a semiconductor device according to the second embodiment will be described.

本実施形態に係る半導体装置の製造方法においては、まず、ダイシングシート付きダイボンドフィルムを準備する(準備する工程)。ダイシングシート付きダイボンドフィルム10、12は、ダイボンドフィルム3、3’上に任意に設けられたセパレータを適宜に剥離して、次の様に使用される。以下では、図3を参照しながらダイシングシート付きダイボンドフィルム10を用いた場合を例にして説明する。   In the method for manufacturing a semiconductor device according to this embodiment, first, a die bond film with a dicing sheet is prepared (preparing step). The die bond films 10 and 12 with a dicing sheet are used as follows after appropriately separating the separator arbitrarily provided on the die bond films 3 and 3 ′. Hereinafter, the case where the die bond film with dicing sheet 10 is used will be described as an example with reference to FIG.

まず、ダイシングシート付きダイボンドフィルム10におけるダイボンドフィルム3の半導体ウェハ貼り付け部分3a上に半導体ウェハ4を圧着し、これを接着保持させて固定する(貼り合わせ工程)。本工程は、圧着ロール等の押圧手段により押圧しながら行う。マウントの際の貼り付け温度は特に限定されず、例えば40〜90℃の範囲内であることが好ましく、40〜80℃の範囲内であることがより好ましい。また、マウントの際の貼り合わせ圧力は特に限定されないが、圧力によりダイボンドフィルム3、3’の粘度を低下させる観点から、0.01〜1MPaの範囲内であることが好ましく、0.1〜0.5MPaの範囲内であることがより好ましい。   First, the semiconductor wafer 4 is pressure-bonded onto the semiconductor wafer bonding portion 3a of the die bond film 3 in the die bond film 10 with a dicing sheet, and this is bonded and held and fixed (bonding step). This step is performed while pressing with a pressing means such as a pressure roll. The attaching temperature at the time of mounting is not specifically limited, For example, it is preferable to exist in the range of 40-90 degreeC, and it is more preferable to exist in the range of 40-80 degreeC. Further, the bonding pressure at the time of mounting is not particularly limited, but from the viewpoint of reducing the viscosity of the die bond films 3 and 3 ′ by the pressure, it is preferably within a range of 0.01 to 1 MPa, and 0.1 to 0 More preferably within the range of 5 MPa.

次に、半導体ウェハ4のダイシングを行う(ダイシング工程)。これにより、半導体ウェハ4を所定のサイズに切断して個片化し、半導体チップ5を製造する。ダイシングの方法は特に限定されないが、例えば半導体ウェハ4の回路面側から常法に従い行われる。また、本工程では、例えばダイシングシート付きダイボンドフィルム10まで切込みを行なうフルカットと呼ばれる切断方式等を採用できる。本工程で用いるダイシング装置としては特に限定されず、従来公知のものを用いることができる。また、半導体ウェハは、ダイシングシート付きダイボンドフィルム10により接着固定されているので、チップ欠けやチップ飛びを抑制できると共に、半導体ウェハ4の破損も抑制できる。   Next, dicing of the semiconductor wafer 4 is performed (dicing process). Thereby, the semiconductor wafer 4 is cut into a predetermined size and separated into individual pieces, and the semiconductor chip 5 is manufactured. Although the method of dicing is not particularly limited, for example, the dicing is performed from the circuit surface side of the semiconductor wafer 4 according to a conventional method. Further, in this step, for example, a cutting method called full cut for cutting up to the die bond film 10 with a dicing sheet can be adopted. It does not specifically limit as a dicing apparatus used at this process, A conventionally well-known thing can be used. Moreover, since the semiconductor wafer is bonded and fixed by the die bond film 10 with a dicing sheet, chip breakage and chip jump can be suppressed, and damage to the semiconductor wafer 4 can be suppressed.

次に、ダイシングシート付きダイボンドフィルム10に接着固定された半導体チップを剥離するために、半導体チップ5のピックアップを行う(ピックアップ工程)。ピックアップの方法としては特に限定されず、従来公知の種々の方法を採用できる。例えば、個々の半導体チップ5をダイシングシート付きダイボンドフィルム10側からニードルによって突き上げ、突き上げられた半導体チップ5をピックアップ装置によってピックアップする方法等が挙げられる。   Next, the semiconductor chip 5 is picked up in order to peel off the semiconductor chip adhered and fixed to the die bond film 10 with a dicing sheet (pickup step). The pickup method is not particularly limited, and various conventionally known methods can be employed. For example, a method of pushing up each semiconductor chip 5 from the die bond film with dicing sheet 10 side with a needle and picking up the pushed semiconductor chip 5 with a pickup device, etc. can be mentioned.

ピックアップ条件としては、チッピング防止の点で、ニードル突き上げ速度を5〜100mm/秒とすることが好ましく、5〜10mm/秒とすることがより好ましい。   As pick-up conditions, the needle push-up speed is preferably 5 to 100 mm / sec, and more preferably 5 to 10 mm / sec in terms of preventing chipping.

ここでピックアップは、粘着剤層2が紫外線硬化型である場合、該粘着剤層2に紫外線を照射した後に行う。これにより、粘着剤層2のダイボンドフィルム3に対する粘着力が低下し、半導体チップ5の剥離が容易になる。その結果、半導体チップ5を損傷させることなくピックアップが可能となる。紫外線照射の際の照射強度、照射時間等の条件は特に限定されず、適宜必要に応じて設定すればよい。また、紫外線照射に使用する光源としては、公知のものを使用することができる。なお、粘着剤層に予め紫外線照射し硬化させておき、この硬化した粘着剤層とダイボンドフィルムとを貼り合わせている場合は、ここでの紫外線照射は不要である。   Here, when the pressure-sensitive adhesive layer 2 is an ultraviolet curable type, the pickup is performed after the pressure-sensitive adhesive layer 2 is irradiated with ultraviolet rays. Thereby, the adhesive force with respect to the die-bonding film 3 of the adhesive layer 2 falls, and peeling of the semiconductor chip 5 becomes easy. As a result, the pickup can be performed without damaging the semiconductor chip 5. Conditions such as irradiation intensity and irradiation time at the time of ultraviolet irradiation are not particularly limited, and may be set as necessary. Moreover, a well-known thing can be used as a light source used for ultraviolet irradiation. In addition, when the adhesive layer is preliminarily irradiated and cured and this cured adhesive layer and the die bond film are bonded together, the ultraviolet irradiation here is unnecessary.

次に、ピックアップした半導体チップ5を、ダイボンドフィルム3を介して被着体6に接着固定する(ダイボンド工程)。被着体6としては、リードフレーム、TABフィルム、基板又は別途作製した半導体チップ等が挙げられる。被着体6は、例えば、容易に変形されるような変形型被着体であってもよく、変形することが困難である非変形型被着体(半導体ウェハ等)であってもよい。   Next, the picked-up semiconductor chip 5 is bonded and fixed to the adherend 6 via the die-bonding film 3 (die-bonding process). Examples of the adherend 6 include a lead frame, a TAB film, a substrate, and a separately manufactured semiconductor chip. The adherend 6 may be, for example, a deformable adherend that can be easily deformed or a non-deformable adherend (such as a semiconductor wafer) that is difficult to deform.

前記基板としては、従来公知のものを使用することができる。また、前記リードフレームとしては、Cuリードフレーム、42Alloyリードフレーム等の金属リードフレームやガラスエポキシ、BT(ビスマレイミド−トリアジン)、ポリイミド等からなる有機基板を使用することができる。しかし、本発明はこれに限定されるものではなく、半導体チップをマウントし、半導体チップと電気的に接続して使用可能な回路基板も含まれる。   A conventionally well-known thing can be used as said board | substrate. As the lead frame, a metal lead frame such as a Cu lead frame or a 42 Alloy lead frame, or an organic substrate made of glass epoxy, BT (bismaleimide-triazine), polyimide, or the like can be used. However, the present invention is not limited to this, and includes a circuit board that can be used by mounting a semiconductor chip and electrically connecting to the semiconductor chip.

次に、ダイボンドフィルム3は熱硬化型であるので、加熱硬化により、半導体チップ5を被着体6に接着固定し、耐熱強度を向上させる(熱硬化工程)。加熱温度は、80〜200℃、好ましくは100〜175℃、より好ましくは100〜140℃で行うことができる。また、加熱時間は、0.1〜24時間、好ましくは0.1〜3時間、より好ましくは0.2〜1時間で行うことができる。また、加熱硬化は、加圧条件下で行なってもよい。加圧条件としては、1〜20kg/cmの範囲内が好ましく、3〜15kg/cmの範囲内がより好ましい。加圧下での加熱硬化は、例えば、不活性ガスを充填したチャンバー内で行なうことができる。なお、ダイボンドフィルム3を介して半導体チップ5が基板等に接着固定されたものは、リフロー工程に供することができる。 Next, since the die bond film 3 is a thermosetting type, the semiconductor chip 5 is bonded and fixed to the adherend 6 by heat curing to improve the heat resistance (thermosetting step). The heating temperature can be 80 to 200 ° C, preferably 100 to 175 ° C, more preferably 100 to 140 ° C. The heating time can be 0.1 to 24 hours, preferably 0.1 to 3 hours, more preferably 0.2 to 1 hour. Moreover, you may perform heat hardening on pressurization conditions. The pressurization condition is preferably in a range of 1~20kg / cm 2, in the range of 3~15kg / cm 2 is more preferable. The heat curing under pressure can be performed, for example, in a chamber filled with an inert gas. In addition, what the semiconductor chip 5 adhere | attached and fixed to the board | substrate etc. via the die-bonding film 3 can use for a reflow process.

熱硬化後のダイボンドフィルム3の剪断接着力は、被着体6に対して0.2MPa以上であることが好ましく、より好ましくは0.2〜10MPaである。ダイボンドフィルム3の剪断接着力が少なくとも0.2MPa以上であると、ワイヤーボンディング工程の際に、当該工程における超音波振動や加熱により、ダイボンドフィルム3と半導体チップ5又は被着体6との接着面でずり変形を生じることがない。すなわち、ワイヤーボンディングの際の超音波振動により半導体チップが動くことがなく、これによりワイヤーボンディングの成功率が低下するのを防止する。   The shear bond strength of the die-bonding film 3 after thermosetting is preferably 0.2 MPa or more with respect to the adherend 6, more preferably 0.2 to 10 MPa. When the shear bond strength of the die bond film 3 is at least 0.2 MPa or more, the bonding surface between the die bond film 3 and the semiconductor chip 5 or the adherend 6 by the ultrasonic vibration or heating in the wire bonding process. No shear deformation occurs. That is, the semiconductor chip does not move due to ultrasonic vibration during wire bonding, thereby preventing the success rate of wire bonding from decreasing.

次に、必要に応じて、図3に示すように、被着体6の端子部(インナーリード)の先端と半導体チップ5上の電極パッド(図示しない)とをボンディングワイヤー7で電気的に接続する(ワイヤーボンディング工程)。前記ボンディングワイヤー7としては、例えば金線、アルミニウム線又は銅線等が用いられる。ワイヤーボンディングを行う際の温度は、80〜250℃、好ましくは80〜220℃の範囲内で行われる。また、その加熱時間は数秒〜数分間行われる。結線は、前記温度範囲内となる様に加熱された状態で、超音波による振動エネルギーと印加加圧による圧着工ネルギーの併用により行われる。本工程は、ダイボンドフィルム3の熱硬化を行うことなく実行することができる。   Next, if necessary, as shown in FIG. 3, the tip of the terminal portion (inner lead) of the adherend 6 and an electrode pad (not shown) on the semiconductor chip 5 are electrically connected by a bonding wire 7. (Wire bonding process). As the bonding wire 7, for example, a gold wire, an aluminum wire, a copper wire or the like is used. The temperature at the time of wire bonding is 80 to 250 ° C, preferably 80 to 220 ° C. The heating time is several seconds to several minutes. The connection is performed by a combination of vibration energy by ultrasonic waves and crimping energy by applying pressure while being heated so as to be within the temperature range. This step can be performed without thermosetting the die bond film 3.

次に、必要に応じて、図3に示すように、封止樹脂8により半導体チップ5を封止する(封止工程)。本工程は、被着体6に搭載された半導体チップ5やボンディングワイヤー7を保護するために行われる。本工程は、封止用の樹脂を金型で成型することにより行うことができる。封止樹脂8としては、例えばエポキシ系の樹脂を使用する。樹脂封止の際の加熱温度は、通常175℃で60〜90秒間行われるが、本発明はこれに限定されず、例えば165〜185℃で、数分間キュアすることができる。これにより、封止樹脂を硬化させると共に、ダイボンドフィルム3を介して半導体チップ5と被着体6とを固着させる。すなわち、本発明においては、後述する後硬化工程が行われない場合においても、本工程においてダイボンドフィルム3による固着が可能であり、製造工程数の減少及び半導体装置の製造期間の短縮に寄与することができる。また、本封止工程では、シート状の封止用シートに半導体チップ5を埋め込む方法(例えば、特開2013−7028号公報参照)を採用することもできる。   Next, as necessary, as shown in FIG. 3, the semiconductor chip 5 is sealed with a sealing resin 8 (sealing step). This step is performed to protect the semiconductor chip 5 and the bonding wire 7 mounted on the adherend 6. This step can be performed by molding a sealing resin with a mold. As the sealing resin 8, for example, an epoxy resin is used. Although the heating temperature at the time of resin sealing is normally performed at 175 degreeC for 60 to 90 second, this invention is not limited to this, For example, it can cure at 165 to 185 degreeC for several minutes. Thereby, the sealing resin is cured, and the semiconductor chip 5 and the adherend 6 are fixed through the die bond film 3. That is, in the present invention, even when the post-curing step described later is not performed, the die-bonding film 3 can be fixed in this step, which contributes to the reduction in the number of manufacturing steps and the manufacturing time of the semiconductor device. Can do. In this sealing step, a method of embedding the semiconductor chip 5 in a sheet-like sealing sheet (see, for example, JP 2013-7028 A) can also be employed.

次に、必要に応じて加熱を行い、前記封止工程で硬化不足の封止樹脂8を完全に硬化させる(後硬化工程)。封止工程においてダイボンドフィルム3が完全に熱硬化していない場合でも、本工程において封止樹脂8と共にダイボンドフィルム3の完全な熱硬化が可能となる。本工程における加熱温度は、封止樹脂の種類により異なるが、例えば165〜185℃の範囲内であり、加熱時間は0.5〜8時間程度である。   Next, heating is performed as necessary to completely cure the insufficiently cured sealing resin 8 in the sealing process (post-curing process). Even when the die bond film 3 is not completely thermoset in the sealing step, the die bond film 3 can be completely thermoset together with the sealing resin 8 in this step. Although the heating temperature in this process changes with kinds of sealing resin, it exists in the range of 165-185 degreeC, for example, and heating time is about 0.5 to 8 hours.

なお、本実施形態に係る半導体装置の製造方法は、ダイボンド工程による仮固着の後、ダイボンドフィルム3の加熱処理による熱硬化工程を経ることなくワイヤーボンディングを行い、さらに半導体チップ5を封止樹脂で封止して、当該封止樹脂を硬化(後硬化)させてもよい。この場合、ダイボンドフィルム3の仮固着時の剪断接着力は、被着体6に対して0.2MPa以上であることが好ましく、より好ましくは0.2〜10MPaである。ダイボンドフィルム3の仮固着時における剪断接着力が少なくとも0.2MPa以上であると、加熱工程を経ることなくワイヤーボンディング工程を行っても、当該工程における超音波振動や加熱により、ダイボンドフィルム3と半導体チップ5又は被着体6との接着面でずり変形を生じることがない。すなわち、ワイヤーボンディングの際の超音波振動により半導体チップが動くことがなく、これによりワイヤーボンディングの成功率が低下するのを防止する。なお、仮固着とは、以降の工程において支障がないように、熱硬化型ダイボンドフィルムの硬化反応を完全に進行した状態に至らない程度で該ダイボンドフィルムを硬化させて(半硬化状態にして)半導体チップ5を固定した状態をいう。なお、ダイボンドフィルムの加熱処理による熱硬化工程を経ることなくワイヤーボンディングを行う場合、上記後硬化させる工程は、本明細書における熱硬化工程に相当する。   In addition, the manufacturing method of the semiconductor device according to the present embodiment performs wire bonding without passing through the thermosetting process by heat treatment of the die bond film 3 after the temporary fixing by the die bonding process, and further, the semiconductor chip 5 is sealed with a sealing resin. It may be sealed and the sealing resin may be cured (post-cured). In this case, the shear adhesive force at the time of temporary fixing of the die bond film 3 is preferably 0.2 MPa or more, more preferably 0.2 to 10 MPa with respect to the adherend 6. Even if the wire bonding step is performed without passing through the heating step, the die bond film 3 and the semiconductor are bonded by the ultrasonic vibration or heating in the step, when the shear bonding force at the time of temporary fixing of the die bond film 3 is at least 0.2 MPa. Shear deformation does not occur on the bonding surface with the chip 5 or the adherend 6. That is, the semiconductor chip does not move due to ultrasonic vibration during wire bonding, thereby preventing the success rate of wire bonding from decreasing. Temporary fixing means that the die-bonding film is cured (in a semi-cured state) to such an extent that the curing reaction of the thermosetting die-bonding film does not proceed completely so as not to hinder the subsequent steps. A state in which the semiconductor chip 5 is fixed. In addition, when performing wire bonding without passing through the thermosetting process by the heat processing of a die-bonding film, the said post-curing process is equivalent to the thermosetting process in this specification.

なお、本発明のダイシングシート付きダイボンドフィルムは、複数の半導体チップを積層して3次元実装をする場合にも好適に用いることができる。このとき、半導体チップ間にダイボンドフィルムとスペーサとを積層させてもよく、スペーサを積層することなく、ダイボンドフィルムのみを半導体チップ間に積層させてもよく、製造条件や用途等に応じて適宜変更可能である。   In addition, the die-bonding film with a dicing sheet of this invention can be used suitably also when laminating | stacking a some semiconductor chip and carrying out three-dimensional mounting. At this time, the die bond film and the spacer may be laminated between the semiconductor chips, or only the die bond film may be laminated between the semiconductor chips without laminating the spacers. Is possible.

以下に、この発明の好適な実施例を例示的に詳しく説明する。ただし、この実施例に記載されている材料や配合量等は、特に限定的な記載がない限りは、この発明の要旨をそれらのみに限定する趣旨のものではない。なお、「部」とあるのは、「重量部」を意味する。   Hereinafter, preferred embodiments of the present invention will be described in detail by way of example. However, the materials, blending amounts, and the like described in the examples are not intended to limit the gist of the present invention only to those unless otherwise specified. “Parts” means “parts by weight”.

(実施例1)
<熱硬化型ダイボンドフィルムの作製>
下記(a)〜(f)をMEK(メチルエチルケトン)に溶解させ、粘度が室温で150mPa・sになるように濃度を調整し、接着剤組成物溶液を得た。
(a)エポキシ樹脂(三菱化学(株)製、製品名:JER827(ビスフェノールA型エポキシ樹脂)、室温で液状(軟化点は25℃以下))
9.5部
(b)フェノール樹脂(ビフェニルアラルキル骨格を有するフェノール樹脂、明和化成社製、製品名:MEH−7851SS、軟化点67℃、水酸基当量203g/eq.)
9.5部
(c)アクリル共重合体(ナガセケムテックス(株)製、製品名:テイサンレジンSG−P3、重量平均分子量:85万、ガラス転移温度:12℃)
1部
(d)硬化促進触媒(北興化学(株)製、製品名:TPP−MK、テトラフェニルホスホニウムテトラ−p−トリボレート)
0.2部
(e)球状アルミナフィラーA(電気化学工業(株)製、製品名:DAW−05、平均粒径:5.1μm、比表面積:0.5m/g)
60部
(f)球状アルミナフィラーB((株)アドマテックス製、製品名:AO802、平均粒径:0.7μm、比表面積:7.5m/g)
20部
Example 1
<Preparation of thermosetting die bond film>
The following (a) to (f) were dissolved in MEK (methyl ethyl ketone), the concentration was adjusted so that the viscosity was 150 mPa · s at room temperature, and an adhesive composition solution was obtained.
(A) Epoxy resin (Mitsubishi Chemical Corporation, product name: JER827 (bisphenol A type epoxy resin), liquid at room temperature (softening point is 25 ° C. or less))
9.5 parts (b) phenolic resin (phenolic resin having a biphenylaralkyl skeleton, manufactured by Meiwa Kasei Co., Ltd., product name: MEH-7851SS, softening point 67 ° C., hydroxyl group equivalent 203 g / eq.)
9.5 parts (c) acrylic copolymer (manufactured by Nagase ChemteX Corporation, product name: Teisan Resin SG-P3, weight average molecular weight: 850,000, glass transition temperature: 12 ° C.)
1 part (d) curing acceleration catalyst (manufactured by Hokuko Chemical Co., Ltd., product name: TPP-MK, tetraphenylphosphonium tetra-p-triborate)
0.2 part (e) spherical alumina filler A (manufactured by Denki Kagaku Kogyo Co., Ltd., product name: DAW-05, average particle size: 5.1 μm, specific surface area: 0.5 m 2 / g)
60 parts (f) spherical alumina filler B (manufactured by Admatechs, product name: AO802, average particle size: 0.7 μm, specific surface area: 7.5 m 2 / g)
20 copies

なお、球状アルミナフィラーA及び球状アルミナフィラーBは、予め表面処理を行なった。表面処理は乾式法で行い、下記式で表される量(シランカップリング剤処理量)のシランカップリング剤で処理した。シランカップリング剤は信越化学のKBM503を用いた。
(シランカップリング剤処理量)=(アルミナフィラーの重量(g)×アルミナフィラーの比表面積(m/g))/シランカップリング剤の最小被覆面積(m/g)
シランカップリング剤の最小被覆面積(m/g)=6.02×1023×13×10−20/シランカップリング剤の分子量
The spherical alumina filler A and the spherical alumina filler B were subjected to surface treatment in advance. The surface treatment was performed by a dry method, and was treated with a silane coupling agent in an amount represented by the following formula (silane coupling agent treatment amount). As a silane coupling agent, Shin-Etsu Chemical KBM503 was used.
(Silane coupling agent treatment amount) = (weight of alumina filler (g) × specific surface area of alumina filler (m 2 / g)) / minimum coating area of silane coupling agent (m 2 / g)
Minimum covering area of silane coupling agent (m 2 /g)=6.02×10 23 × 13 × 10 −20 / Molecular weight of silane coupling agent

この接着剤組成物溶液を、シリコーン離型処理した厚さが50μmのポリエチレンテレフタレートフィルムからなる離型処理フィルム(剥離ライナー)上に塗布した後、130℃で2分間乾燥させた。これにより厚さ25μmのダイボンドフィルムAを作製した。   The adhesive composition solution was applied on a release film (release liner) made of a polyethylene terephthalate film having a thickness of 50 μm after the silicone release treatment, and then dried at 130 ° C. for 2 minutes. Thus, a die bond film A having a thickness of 25 μm was produced.

(実施例2)
<熱硬化型ダイボンドフィルムの作製>
下記(a)〜(f)をMEK(メチルエチルケトン)に溶解させ、粘度が室温150mPa・sになるように濃度を調整し、接着剤組成物溶液を得た。
(a)エポキシ樹脂(三菱化学(株)製、製品名:JER827(ビスフェノールA型エポキシ樹脂)、室温で液状(軟化点は25℃以下))
6.5部
(b)フェノール樹脂(ビフェニルアラルキル骨格を有するフェノール樹脂、明和化成社製、製品名:MEH−7851SS、軟化点67℃、水酸基当量203g/eq.)
7部
(c)アクリル共重合体(ナガセケムテックス(株)製、製品名:テイサンレジンSG−P3、重量平均分子量:85万、ガラス転移温度:12℃)
1.5部
(d)硬化促進触媒(北興化学(株)製、製品名:TPP−MK、テトラフェニルホスホニウムテトラ−p−トリボレート)
0.15部
(e)球状アルミナフィラーA(電気化学工業(株)製、製品名:DAW−05、平均粒径:5.1μm、比表面積:0.5m/g)
60部
(f)球状アルミナフィラーB((株)アドマテックス製、製品名:AO802、平均粒径:0.7μm、比表面積:7.5m/g)
25部
(Example 2)
<Preparation of thermosetting die bond film>
The following (a) to (f) were dissolved in MEK (methyl ethyl ketone), the concentration was adjusted so that the viscosity was 150 mPa · s at room temperature, and an adhesive composition solution was obtained.
(A) Epoxy resin (Mitsubishi Chemical Corporation, product name: JER827 (bisphenol A type epoxy resin), liquid at room temperature (softening point is 25 ° C. or less))
6.5 parts (b) phenol resin (phenol resin having biphenyl aralkyl skeleton, manufactured by Meiwa Kasei Co., Ltd., product name: MEH-7851SS, softening point 67 ° C., hydroxyl group equivalent 203 g / eq.)
7 parts (c) acrylic copolymer (manufactured by Nagase ChemteX Corporation, product name: Teisan Resin SG-P3, weight average molecular weight: 850,000, glass transition temperature: 12 ° C.)
1.5 parts (d) curing accelerating catalyst (manufactured by Hokuko Chemical Co., Ltd., product name: TPP-MK, tetraphenylphosphonium tetra-p-triborate)
0.15 parts (e) spherical alumina filler A (manufactured by Denki Kagaku Kogyo Co., Ltd., product name: DAW-05, average particle size: 5.1 μm, specific surface area: 0.5 m 2 / g)
60 parts (f) spherical alumina filler B (manufactured by Admatechs, product name: AO802, average particle size: 0.7 μm, specific surface area: 7.5 m 2 / g)
25 copies

なお、球状アルミナフィラーA及び球状アルミナフィラーBは、予め表面処理を行なった。表面処理は乾式法で行い、下記式で表される量(シランカップリング剤処理量)のシランカップリング剤で処理した。シランカップリング剤は信越化学のKBM503を用いた。
(シランカップリング剤処理量)=(アルミナフィラーの重量(g)×アルミナフィラーの比表面積(m/g))/シランカップリング剤の最小被覆面積(m/g)
シランカップリング剤の最小被覆面積(m/g)=6.02×1023×13×10−20/シランカップリング剤の分子量
The spherical alumina filler A and the spherical alumina filler B were subjected to surface treatment in advance. The surface treatment was performed by a dry method, and was treated with a silane coupling agent in an amount represented by the following formula (silane coupling agent treatment amount). As a silane coupling agent, Shin-Etsu Chemical KBM503 was used.
(Silane coupling agent treatment amount) = (weight of alumina filler (g) × specific surface area of alumina filler (m 2 / g)) / minimum coating area of silane coupling agent (m 2 / g)
Minimum covering area of silane coupling agent (m 2 /g)=6.02×10 23 × 13 × 10 −20 / Molecular weight of silane coupling agent

この接着剤組成物溶液を、シリコーン離型処理した厚さが50μmのポリエチレンテレフタレートフィルムからなる離型処理フィルム(剥離ライナー)上に塗布した後、130℃で2分間乾燥させた。これにより、厚さ25μmのダイボンドフィルムBを作製した。   The adhesive composition solution was applied on a release film (release liner) made of a polyethylene terephthalate film having a thickness of 50 μm after the silicone release treatment, and then dried at 130 ° C. for 2 minutes. Thus, a die bond film B having a thickness of 25 μm was produced.

(比較例1)
<熱硬化型ダイボンドフィルムの作製>
下記(a)〜(e)をMEK(メチルエチルケトン)に溶解させ、粘度が室温で150mPa・sになるように濃度を調整し、接着剤組成物溶液を得た。
(a)エポキシ樹脂(三菱化学(株)製、製品名:JER827(ビスフェノールA型エポキシ樹脂)、室温で液状(軟化点は25℃以下))
8部
(b)フェノール樹脂(ビフェニルアラルキル骨格を有するフェノール樹脂、明和化成社製、製品名:MEH−7851SS、軟化点67℃、水酸基当量203g/eq.)
8部
(c)アクリル共重合体(ナガセケムテックス(株)製、製品名:テイサンレジンSG−P3、重量平均分子量:85万、ガラス転移温度:12℃)
4部
(d)硬化促進触媒(北興化学(株)製、製品名:TPP−MK、テトラフェニルホスホニウムテトラ−p−トリボレート)
0.2部
(e)球状アルミナフィラーB((株)アドマテックス製、製品名:AO802、平均粒径:0.7μm、比表面積:7.5m/g)
80部
(Comparative Example 1)
<Preparation of thermosetting die bond film>
The following (a) to (e) were dissolved in MEK (methyl ethyl ketone), the concentration was adjusted so that the viscosity was 150 mPa · s at room temperature, and an adhesive composition solution was obtained.
(A) Epoxy resin (Mitsubishi Chemical Corporation, product name: JER827 (bisphenol A type epoxy resin), liquid at room temperature (softening point is 25 ° C. or less))
8 parts (b) phenol resin (phenol resin having biphenyl aralkyl skeleton, manufactured by Meiwa Kasei Co., Ltd., product name: MEH-7851SS, softening point 67 ° C., hydroxyl group equivalent 203 g / eq.)
8 parts (c) acrylic copolymer (manufactured by Nagase ChemteX Corporation, product name: Teisan Resin SG-P3, weight average molecular weight: 850,000, glass transition temperature: 12 ° C.)
4 parts (d) curing accelerating catalyst (manufactured by Hokuko Chemical Co., Ltd., product name: TPP-MK, tetraphenylphosphonium tetra-p-triborate)
0.2 part (e) spherical alumina filler B (manufactured by Admatechs, product name: AO802, average particle size: 0.7 μm, specific surface area: 7.5 m 2 / g)
80 copies

なお、球状アルミナフィラーBは、予め表面処理を行なった。表面処理は乾式法で行い、下記式で表される量(シランカップリング剤処理量)のシランカップリング剤で処理した。シランカップリング剤は信越化学のKBM503を用いた。
(シランカップリング剤処理量)=(アルミナフィラーの重量(g)×アルミナフィラーの比表面積(m/g))/シランカップリング剤の最小被覆面積(m/g)
シランカップリング剤の最小被覆面積(m/g)=6.02×1023×13×10−20/シランカップリング剤の分子量
The spherical alumina filler B was subjected to surface treatment in advance. The surface treatment was performed by a dry method, and was treated with a silane coupling agent in an amount represented by the following formula (silane coupling agent treatment amount). As a silane coupling agent, Shin-Etsu Chemical KBM503 was used.
(Silane coupling agent treatment amount) = (weight of alumina filler (g) × specific surface area of alumina filler (m 2 / g)) / minimum coating area of silane coupling agent (m 2 / g)
Minimum covering area of silane coupling agent (m 2 /g)=6.02×10 23 × 13 × 10 −20 / Molecular weight of silane coupling agent

この接着剤組成物溶液を、シリコーン離型処理した厚さが50μmのポリエチレンテレフタレートフィルムからなる離型処理フィルム(剥離ライナー)上に塗布した後、130℃で2分間乾燥させた。これにより、厚さ25μmのダイボンドフィルムCを作製した。   The adhesive composition solution was applied on a release film (release liner) made of a polyethylene terephthalate film having a thickness of 50 μm after the silicone release treatment, and then dried at 130 ° C. for 2 minutes. Thus, a die bond film C having a thickness of 25 μm was produced.

なお、実施例、比較例に係るダイボンドフィルムにおけるフィラー全体(球状アルミナフィラーA及び球状アルミナフィラーB)の平均粒径、及び、フィラー全体の比表面積は、表1に示す通りである。また、A/Bの値、ダイボンドフィルム全体に対するフィラーの充填量、樹脂成分中(熱硬化性樹脂と熱可塑性樹脂の合計量中)の熱硬化性樹脂の割合、樹脂成分中(熱硬化性樹脂と熱可塑性樹脂の合計量中)の熱可塑性樹脂の割合、も合わせて表1に示した。   In addition, the average particle diameter of the whole filler (spherical alumina filler A and spherical alumina filler B) in the die-bonding films according to Examples and Comparative Examples and the specific surface area of the whole filler are as shown in Table 1. Moreover, the value of A / B, the filling amount of the filler with respect to the whole die bond film, the ratio of the thermosetting resin in the resin component (in the total amount of the thermosetting resin and the thermoplastic resin), the resin component (the thermosetting resin) Table 1 also shows the ratio of the thermoplastic resin in the total amount of and the thermoplastic resin).

(130℃における高速せん断時(ずり速度50(1/秒))の溶融粘度測定)
ダイボンドフィルムA〜Cの熱硬化前の130℃における高速せん断時の溶融粘度を測定した。測定にはレオメーター(HAAKE社製、RS−1)を用いて、パラレルプレート法により行った。即ち、各ダイボンドフィルムA〜Cから0.1gを採取して試料とし、この試料を予め130℃に熱してあるプレートに仕込んだ。溶融粘度は測定開始から300秒後の値とした。また、ずり速度を50(1/秒)、プレート間のギャップは0.1mmとした。結果を下記表1に示す。
(Measurement of melt viscosity at high shear at 130 ° C. (shear rate 50 (1 / second))
The melt viscosity during high-speed shearing at 130 ° C. before thermosetting of the die bond films A to C was measured. The measurement was performed by a parallel plate method using a rheometer (manufactured by HAAKE, RS-1). That is, 0.1 g from each of the die bond films A to C was sampled and used as a sample, and this sample was loaded on a plate heated to 130 ° C. in advance. The melt viscosity was a value 300 seconds after the start of measurement. The shear rate was 50 (1 / second), and the gap between the plates was 0.1 mm. The results are shown in Table 1 below.

(130℃における低速せん断時(ずり速度5(1/秒))の溶融粘度測定)
ダイボンドフィルムA〜Cの熱硬化前の130℃における低速せん断時の溶融粘度を測定した。測定にはレオメーター(HAAKE社製、RS−1)を用いて、パラレルプレート法により行った。即ち、各ダイボンドフィルムA〜Cから0.1gを採取して試料とし、この試料を予め130℃に熱してあるプレートに仕込んだ。溶融粘度は測定開始から300秒後の値とした。また、ずり速度を5(1/秒)、プレート間のギャップは0.1mmとした。結果を下記表1に示す。
(Measurement of melt viscosity at low shear at 130 ° C (shear rate 5 (1 / second))
The melt viscosity at the time of low-speed shearing at 130 ° C. before thermosetting of the die bond films A to C was measured. The measurement was performed by a parallel plate method using a rheometer (manufactured by HAAKE, RS-1). That is, 0.1 g from each of the die bond films A to C was sampled and used as a sample, and this sample was loaded on a plate heated to 130 ° C. in advance. The melt viscosity was a value 300 seconds after the start of measurement. The shear rate was 5 (1 / second), and the gap between the plates was 0.1 mm. The results are shown in Table 1 below.

(熱伝導率の測定)
ダイボンドフィルムA〜Cの熱硬化後の熱伝導率の測定を行なった。熱伝導率は下記の式から求めた。結果を表1に示す。なお、熱硬化後の熱伝導率とは、130℃で1時間加熱し、続いて、175℃で5時間加熱した後の熱伝導率である。
(熱伝導率)=(熱拡散係数)×(比熱)×(比重)
(Measurement of thermal conductivity)
The thermal conductivity after thermosetting of the die bond films A to C was measured. The thermal conductivity was obtained from the following formula. The results are shown in Table 1. In addition, the heat conductivity after thermosetting is a heat conductivity after heating at 130 degreeC for 1 hour, and subsequently heating at 175 degreeC for 5 hours.
(Thermal conductivity) = (thermal diffusion coefficient) x (specific heat) x (specific gravity)

<熱拡散係数>.
ダイボンドフィルムを1mm厚に積層したのち、直径1cmの円形形状に打ち抜いた。次に、130℃で1時間加熱し、続いて、175℃で5時間加熱した。このサンプルを用いて、レーザーフラッシュ法熱測定装置装置(アルバック社製、TC−9000)を用いて熱拡散係数を測定した。
<Thermal diffusion coefficient>.
After the die bond film was laminated to a thickness of 1 mm, it was punched into a circular shape having a diameter of 1 cm. Next, it was heated at 130 ° C. for 1 hour, and subsequently heated at 175 ° C. for 5 hours. Using this sample, the thermal diffusion coefficient was measured using a laser flash method thermal measurement apparatus (manufactured by ULVAC, TC-9000).

<比熱>
DSC(TA instrument製、Q−2000)を用いてJIS−7123の規格に沿った測定方法によって求めた。
<Specific heat>
It calculated | required by the measuring method according to the specification of JIS-7123 using DSC (The product made from TA instrument, Q-2000).

<比重>
電子天秤((株)島津製作所製、AEL−200)を用いてアルキメデス法によって測定した。
<Specific gravity>
Measurement was performed by the Archimedes method using an electronic balance (manufactured by Shimadzu Corporation, AEL-200).

(ボイド評価)
熱ラミネートを用いて、厚さ25μmのダイボンドフィルムA〜Cを、厚さ100μmのガラスチップに、10mm×10mmの面積で貼りつけて、サンプルチップを作成した。貼り付け時の温度は60℃、圧力は0.15MPaとした。
次に、サンプルチップをBGA基板(日本サーキット工業(株)社製、製品名:CA−BGA(2)、表面十点平均粗さ(Rz)=11〜13μm)に130℃、2kg、2秒間の条件でボンディングを行った。その後、加圧条件下で130℃で1時間加熱し、続いて、175℃で5時間加熱した。加熱硬化時の加圧は、具体的には、オーブン内に窒素ガスを5kg/cmで充てんすることで行った。ボンディングしたサンプルチップのガラス面側から光学顕微鏡を用いて観察した。観察画像においてボイドが占める面積を二値化ソフト(WinRoofver.5.6)を用いて算出した。ボイドの占める面積がダイボンドフィルムの表面積に対して20%未満であった場合を「○」、20%以上であった場合を「×」として評価した。結果を表1に示す。
(Void evaluation)
Using a thermal laminate, the die bond films A to C having a thickness of 25 μm were attached to a glass chip having a thickness of 100 μm with an area of 10 mm × 10 mm to prepare a sample chip. The temperature at the time of pasting was 60 ° C., and the pressure was 0.15 MPa.
Next, the sample chip was placed on a BGA substrate (manufactured by Nippon Circuit Industry Co., Ltd., product name: CA-BGA (2), surface 10-point average roughness (Rz) = 11 to 13 μm) at 130 ° C., 2 kg, 2 seconds. Bonding was performed under the following conditions. Then, it heated at 130 degreeC on pressurization conditions for 1 hour, followed by heating at 175 degreeC for 5 hours. Specifically, the pressurization at the time of heat curing was performed by filling the oven with nitrogen gas at 5 kg / cm 2 . It observed using the optical microscope from the glass surface side of the bonded sample chip | tip. The area occupied by the void in the observed image was calculated using binarization software (WinRoofer. 5.6). The case where the void occupied area was less than 20% with respect to the surface area of the die bond film was evaluated as “◯”, and the case where it was 20% or more was evaluated as “x”. The results are shown in Table 1.

Figure 2015103573
Figure 2015103573

1 基材
2 粘着剤層
3、3’ ダイボンドフィルム(熱硬化型ダイボンドフィルム)
4 半導体ウェハ
5 半導体チップ
6 被着体
7 ボンディングワイヤー
8 封止樹脂
10、12 ダイシングシート付きダイボンドフィルム
11 ダイシングシート
DESCRIPTION OF SYMBOLS 1 Base material 2 Adhesive layer 3, 3 'Die bond film (thermosetting type die bond film)
4 Semiconductor wafer 5 Semiconductor chip 6 Substrate 7 Bonding wire 8 Sealing resin 10, 12 Die bond film with dicing sheet 11 Dicing sheet

Claims (8)

熱硬化後の熱伝導率が1W/m・K以上であり、
熱伝導率が12W/m・K以上の熱伝導性粒子を、熱硬化型ダイボンドフィルム全体に対して75重量%以上含有しており、
130℃において、ずり速度50(1/秒)で測定される溶融粘度が200Pa・s以下であることを特徴とする熱硬化型ダイボンドフィルム。
The thermal conductivity after thermosetting is 1 W / m · K or more,
Containing 75% by weight or more of thermally conductive particles having a thermal conductivity of 12 W / m · K or more with respect to the entire thermosetting die-bonding film;
A thermosetting die-bonding film having a melt viscosity of 200 Pa · s or less measured at a shear rate of 50 (1 / second) at 130 ° C.
前記熱伝導性粒子の平均粒径が、1μm以上10μm以下であることを特徴とする請求項1に記載の熱硬化型ダイボンドフィルム。   2. The thermosetting die-bonding film according to claim 1, wherein the heat conductive particles have an average particle size of 1 μm to 10 μm. 熱可塑性樹脂と熱硬化性樹脂とを含有し、
前記熱硬化性樹脂の含有重量部をAとし、前記熱可塑性樹脂の含有重量部をBとしたときに、A/Bが5以上であることを特徴とする請求項1又は2に記載の熱硬化型ダイボンドフィルム。
Containing a thermoplastic resin and a thermosetting resin,
The heat according to claim 1 or 2, wherein A / B is 5 or more, where A is a content part by weight of the thermosetting resin and B is a content part by weight of the thermoplastic resin. Cured die bond film.
前記熱硬化性樹脂は、軟化点が100℃以下のものを含むことを特徴とする請求項3に記載の熱硬化型ダイボンドフィルム。   The thermosetting die-bonding film according to claim 3, wherein the thermosetting resin includes a softening point of 100 ° C. or less. 前記熱硬化性樹脂は、室温で液状のものを含むことを特徴とする請求項3又は4に記載の熱硬化型ダイボンドフィルム。   The thermosetting die-bonding film according to claim 3 or 4, wherein the thermosetting resin includes a liquid at room temperature. 請求項1〜5のいずれか1に記載の熱硬化型ダイボンドフィルムを準備する工程と、
前記熱硬化型ダイボンドフィルムを介して、半導体チップを被着体上にダイボンドするダイボンド工程とを含むことを特徴とする半導体装置の製造方法。
Preparing the thermosetting die-bonding film according to any one of claims 1 to 5,
A die bonding step of die-bonding a semiconductor chip on an adherend through the thermosetting die-bonding film.
請求項1〜5のいずれか1に記載の熱硬化型ダイボンドフィルムが、基材上に粘着剤層が積層されたダイシングシート上に積層されていることを特徴とするダイシングシート付きダイボンドフィルム。   A die-bonding film with a dicing sheet, wherein the thermosetting die-bonding film according to claim 1 is laminated on a dicing sheet in which an adhesive layer is laminated on a substrate. 請求項7に記載のダイシングシート付きダイボンドフィルムを準備する工程と、
前記ダイシングシート付きダイボンドフィルムの熱硬化型ダイボンドフィルムと、半導体ウェハの裏面とを貼り合わせる貼り合わせ工程と、
前記半導体ウェハを前記熱硬化型ダイボンドフィルムと共にダイシングして、チップ状の半導体チップを形成するダイシング工程と、
前記半導体チップを、前記ダイシングシート付きダイボンドフィルムから前記熱硬化型ダイボンドフィルムと共にピックアップするピックアップ工程と、
前記熱硬化型ダイボンドフィルムを介して、前記半導体チップを被着体上にダイボンドするダイボンド工程とを含むことを特徴とする半導体装置の製造方法。
Preparing a die bond film with a dicing sheet according to claim 7;
A bonding step of bonding the thermosetting die-bonding film of the die-bonding film with the dicing sheet and the back surface of the semiconductor wafer;
Dicing the semiconductor wafer together with the thermosetting die bond film to form a chip-shaped semiconductor chip;
A pick-up step of picking up the semiconductor chip together with the thermosetting die-bonding film from the die-bonding film with the dicing sheet;
A die-bonding step of die-bonding the semiconductor chip onto an adherend through the thermosetting die-bonding film.
JP2013241284A 2013-06-04 2013-11-21 Thermosetting die bond film, die bond film with dicing sheet and method for manufacturing semiconductor device Pending JP2015103573A (en)